Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Arkema Group Orevac® 9314 Film EVA-MAH Terpolymer

Category Polymer , Film , Thermoplastic , Ethylene Vinyl Acetate
Manufacturer Arkema
Trade Name OREVAC®
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Arkema Group Orevac® 9314 Film EVA-MAH Terpolymer.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
EVA Terpolymers based Main Application: Blown film coextrusionInformation provided by Arkema Group
Physical Properties Metric English Comments
Density 0.940 g/cc
0.0340 lb/in³
ASTM D1505
Vinyl Acetate Content 13 - 14 %
13 - 14 %
Melt Flow 1.5 - 2.5 g/10 min

@Load 2.16 kg,
Temperature 190 °C
1.5 - 2.5 g/10 min

@Load 4.76 lb,
Temperature 374 °F
ASTM D1238
Mechanical Properties Metric English Comments
Hardness, Shore D 33.7
33.7
ISO 868
Tensile Strength at Break 27.7 MPa
4020 psi
50 microns film; ASTM D882
Tensile Strength, Yield 5.30 MPa
769 psi
50 microns film; ASTM D882
Elongation at Break 570 %
570 %
50 microns film; ASTM D882
Modulus of Elasticity 0.0547 GPa
7.93 ksi
ISO R527
Dart Drop Test 365 g
0.805 lb
50 microns film
Thermal Properties Metric English Comments
Melting Point 90.0 °C
194 °F
D.S.C. method
Vicat Softening Point 70.0 °C
158 °F
ASTM D1525
Optical Properties Metric English Comments
Haze 10.2 %
10.2 %
50 micron film; ASTM D1003
Users viewing this material also viewed the following:
Copyright © lookpolymers.com All Rights Reserved