ExxonMobil Exceed™ 1015HA Metallocene Polyethylene Resin

Category Polymer , Thermoplastic , Polyethylene (PE)
Manufacturer Exxon Chemical
Trade Name Exceed™
Port Shanghai port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF ExxonMobil Exceed™ 1015HA Metallocene Polyethylene Resin.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
Product Description: Exceed 1015 mVLDPE resin is metallocene ethylene-hexene copolymer. Films made from Exceed 1015 mVLDPE have outstanding cold temperature toughness, impact strength and puncture. These superior strength properties, along with excellent heat sealing and hot tack performance, make this a very versatile packaging film resin. Availability: Latin America, North America and South AmericaAdditive:Antiblock: NoSlip: NoProcessing Aid: YesThermal Stabilizer: YesApplications:Bag in BoxBarrier Food PackagingBlown FilmFood packagingForm Fill and Seal PackagingFreezer FilmHeavy Duty BagsIce BagsLamination FilmMultilayer Packaging Film Stand Up Pouches Information provided by ExxonMobil
Physical Properties Metric English Comments
Density 0.915 g/cc
0.0331 lb/in³
ExxonMobil method
Melt Flow 1.0 g/10 min

@Load 2.16 kg,
Temperature 190 °C
1.0 g/10 min

@Load 4.76 lb,
Temperature 374 °F
ASTM D1238
Mechanical Properties Metric English Comments
Film Tensile Strength at Yield, MD 8.27 MPa
1200 psi
ASTM D882
Film Tensile Strength at Yield, TD 8.27 MPa
1200 psi
ASTM D882
Film Elongation at Break, MD 470 %
470 %
ASTM D882
Film Elongation at Break, TD 620 %
620 %
ASTM D882
Puncture Energy 4.52 J
3.33 ft-lb
ExxonMobil Method
Elmendorf Tear Strength MD 210 g
210 g
ASTM D1922
Elmendorf Tear Strength TD 360 g
360 g
ASTM D1922
Dart Drop Test 740 g
1.63 lb
ASTM D1709
Film Tensile Strength at Break, MD 64.1 MPa
9300 psi
ASTM D882
Film Tensile Strength at Break, TD 56.5 MPa
8200 psi
ASTM D882
1% Secant Modulus, MD 145 MPa
21000 psi
ASTM D882
1% Secant Modulus, TD 165 MPa
24000 psi
ASTM D882
Thermal Properties Metric English Comments
Melting Point <= 242 °C
<= 468 °F
Peak Melting Point; ExxonMobil method
Optical Properties Metric English Comments
Haze 22 %
22 %
ASTM D1003
Gloss 33 %
33 %
45°; ASTM D2457
Descriptive Properties Value Comments
Puncture Force 12 lbf
ExxonMobil Method