Material Notes:
Description: Curon 14 S is a dense, strong and abrasion resistant castable. Because of the very low percentage of Fe2O3 and SiO2 it is used for highly abrasive conditions in reducing atmospheres.Remarks: These values apply to cast products. Also available in gunning variety, marked "GM".Information provided by Gouda Vuurvast.
Physical Properties Metric English Comments
Bulk Density 2.50 - 2.60 g/cc
0.0903 - 0.0939 lb/in³
After drying at 110°C
Particle Size <= 6000 µm
<= 6000 µm
Grain Size
Mechanical Properties Metric English Comments
Compressive Strength 55.0 - 65.0 MPa

@Temperature 1300 °C
7980 - 9430 psi

@Temperature 2370 °F
Cold Crushing Strength
75.0 - 85.0 MPa

@Temperature 100 °C
10900 - 12300 psi

@Temperature 212 °F
Cold Crushing Strength
Thermal Properties Metric English Comments
Thermal Conductivity 0.780 - 0.880 W/m-K

@Temperature 100 °C
5.41 - 6.11 BTU-in/hr-ft²-°F

@Temperature 212 °F
0.870 - 0.970 W/m-K

@Temperature 600 °C
6.04 - 6.73 BTU-in/hr-ft²-°F

@Temperature 1110 °F
1.03 - 1.13 W/m-K

@Temperature 1300 °C
7.15 - 7.84 BTU-in/hr-ft²-°F

@Temperature 2370 °F
Maximum Service Temperature, Air 1400 °C
2550 °F
Shrinkage -0.800 - 0.800 %

@Temperature 1300 °C
-0.800 - 0.800 %

@Temperature 2370 °F
Permanent Linear Change
Component Elements Properties Metric English Comments
Al2O3 76 %
76 %
Fe2O3 <= 0.50 %
<= 0.50 %
SiO2 <= 2.0 %
<= 2.0 %
Descriptive Properties Value Comments
ASTM Classification C
Material Consumption per 1 m3 2450 kg
Mixing Water 8-10 liters
per 100 kgs dry material