Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Industeel VIRGO 39 16% Cr, 5% Ni, Martensitic Stainless Steel

Category Metal , Ferrous Metal , Martensitic , Stainless Steel
Manufacturer Groupe Arcelor
Trade Name VIRGO
Port Shanghai port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Industeel VIRGO 39 16% Cr, 5% Ni, Martensitic Stainless Steel.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
Description: Virgo 39 is a 16% Cr, 5% Ni, 1% Mo low carbon martensitic stainless steel. The grade is specially designed to combine high mechanical properties including toughness and improved corrosion resistance properties when compared to other martensitic stainless steels, like 13 Cr and 13 Cr 4 Ni grades. The alloy has been primarily designed to resist to erosion-corrosion or cavitation encountered in hydraulic applications. The alloy is also used for hydrofoils legs, as anti-seismic compounds or offshore structures, boats, landing grids for helicopters… where the combined mechanical and corrosion resistance properties are needed. Mining, cement plants, and hydraulic applications take also advantage of its combined abrasion-corrosion resistance properties.Information provided by manufacturer.
Physical Properties Metric English Comments
Density 7.70 g/cc
0.278 lb/in³
Mechanical Properties Metric English Comments
Hardness, Brinell 230 - 320
230 - 320
Typical
Tensile Strength, Ultimate 850 MPa
123000 psi
Quenched Tempered
Tensile Strength, Yield 615 MPa

@Strain 0.200 %
89200 psi

@Strain 0.200 %
Quenched Tempered
Elongation at Break >= 15 %
>= 15 %
Modulus of Elasticity 210 GPa
30500 ksi
Poissons Ratio 0.346
0.346
Calculated
Shear Modulus 78.0 GPa

@Temperature 20.0 °C
11300 ksi

@Temperature 68.0 °F
Charpy Impact 35.0 J
25.8 ft-lb
Guaranteed in T Direction
60.0 J
44.3 ft-lb
Guaranteed in L Direction
100 J
73.8 ft-lb
Typical
Thermal Properties Metric English Comments
CTE, linear 10.0 µm/m-°C

@Temperature 20.0 - 100 °C
5.56 µin/in-°F

@Temperature 68.0 - 212 °F
11.0 µm/m-°C

@Temperature 20.0 - 200 °C
6.11 µin/in-°F

@Temperature 68.0 - 392 °F
Specific Heat Capacity 0.460 J/g-°C

@Temperature 20.0 °C
0.110 BTU/lb-°F

@Temperature 68.0 °F
Thermal Conductivity 20.0 W/m-K

@Temperature 20.0 °C
139 BTU-in/hr-ft²-°F

@Temperature 68.0 °F
Component Elements Properties Metric English Comments
Carbon, C 0.045 %
0.045 %
Chromium, Cr 16 %
16 %
Iron, Fe 77.934 %
77.934 %
As remainder
Molybdenum, Mo 1.0 %
1.0 %
Nickel, Ni 5.0 %
5.0 %
Phosphorous, P 0.020 %
0.020 %
Sulfur, S 0.0010 %
0.0010 %
Electrical Properties Metric English Comments
Electrical Resistivity 0.0000750 ohm-cm

@Temperature 20.0 °C
0.0000750 ohm-cm

@Temperature 68.0 °F
Users viewing this material also viewed the following: