Material Notes:
Description: SBR 1778 is an oil extended cold polymerization SBR with 37.5 parts of discoloring paraffinic/naphthenic oil and light colored high molecular weight styrene-butadiene copolymer of 23.5% bound styrene. SBR 1778 combines the physical properties of oil extended polymers with the light color properties of naphthenic oil.Applications: SBR 1778 can be used to hose, conveyor belt, tire and other industrial products for the light colored goods.CAS No: 9003-55-8Information provided by LG Chemical
Physical Properties Metric English Comments
Specific Gravity 0.920 g/cc
0.920 g/cc
Volatiles 0.30 %
0.30 %
Mooney Viscosity 46

@Temperature 100 °C
46

@Temperature 212 °F
ML 1+4
Ash 0.20 %
0.20 %
Mechanical Properties Metric English Comments
Tensile Strength at Break 22.6 MPa

@Temperature 145 °C,
Time 2100 sec
3280 psi

@Temperature 293 °F,
Time 0.583 hour
ASTM D412
Elongation at Break 500 %

@Temperature 145 °C,
Time 2100 sec
500 %

@Temperature 293 °F,
Time 0.583 hour
ASTM D412
300% Modulus 0.0123 GPa

@Temperature 145 °C,
Time 2100 sec
1.78 ksi

@Temperature 293 °F,
Time 0.583 hour
ASTM D412
Chemical Properties Metric English Comments
Styrene Content 23.5 %
23.5 %
Bound
Descriptive Properties Value Comments
Color Light Tan Bale
Components HAF
68.75, ASTM D3185
SBR 1739
137.5, ASTM D3185
Stearic Acid
1, ASTM D3185
Sulfur
1.75, ASTM D3185
TBBS
1.38, ASTM D3185
ZnO
3, ASTM D3185
Oil Analysis 0.273
Organic Acid 0.05
Soap 0.001