Material Notes:
EVA film for encapsulating solar module Lushan series with ultra fast cure characteristic is used as encapsulate materials for photovoltaic industry. With Innovative technology, Lushan ultra fast cure solar EVA film has developed to be a stable, high properties, and reputable products, and widely used in China and overseas market. Lushan ultra fast cure solar EVA film has very good processing properties that helps PV module manufactures with the most effective production way and save the cost as much as possible.Information provided by Lushan
Processing Properties Metric English Comments
Gel Time 0.000 min

@Temperature 135 °C
0.000 min

@Temperature 275 °F
0% Gel content
0.000 min

@Temperature 138 °C
0.000 min

@Temperature 280 °F
0% Gel content
0.000 min

@Temperature 140 °C
0.000 min

@Temperature 284 °F
0.02% Gel content
0.000 min

@Temperature 143 °C
0.000 min

@Temperature 289 °F
0.09% Gel content
0.000 min

@Temperature 145 °C
0.000 min

@Temperature 293 °F
0.21% Gel content
0.000 min

@Temperature 148 °C
0.000 min

@Temperature 298 °F
1.6% Gel content
0.000 min

@Temperature 150 °C
0.000 min

@Temperature 302 °F
3.59% Gel content
0.000 min

@Temperature 153 °C
0.000 min

@Temperature 307 °F
42.8% Gel content
0.000 min

@Temperature 155 °C
0.000 min

@Temperature 311 °F
61.11% Gel content
3.00 min

@Temperature 135 °C
3.00 min

@Temperature 275 °F
0% Gel content
3.00 min

@Temperature 138 °C
3.00 min

@Temperature 280 °F
23.17% Gel content
3.00 min

@Temperature 140 °C
3.00 min

@Temperature 284 °F
25.7% Gel content
3.00 min

@Temperature 143 °C
3.00 min

@Temperature 289 °F
53.3% Gel content
3.00 min

@Temperature 145 °C
3.00 min

@Temperature 293 °F
43.5% Gel content
3.00 min

@Temperature 148 °C
3.00 min

@Temperature 298 °F
71.81% Gel content
3.00 min

@Temperature 150 °C
3.00 min

@Temperature 302 °F
79.16% Gel content
3.00 min

@Temperature 153 °C
3.00 min

@Temperature 307 °F
80.27% Gel content
3.00 min

@Temperature 155 °C
3.00 min

@Temperature 311 °F
83.62% Gel content
5.00 min

@Temperature 135 °C
5.00 min

@Temperature 275 °F
3.39% Gel content
5.00 min

@Temperature 138 °C
5.00 min

@Temperature 280 °F
46.51% Gel content
5.00 min

@Temperature 140 °C
5.00 min

@Temperature 284 °F
53.77% Gel content
5.00 min

@Temperature 143 °C
5.00 min

@Temperature 289 °F
71.9% Gel content
5.00 min

@Temperature 145 °C
5.00 min

@Temperature 293 °F
70.85% Gel content
5.00 min

@Temperature 148 °C
5.00 min

@Temperature 298 °F
81.33% Gel content
5.00 min

@Temperature 150 °C
5.00 min

@Temperature 302 °F
84.59% Gel content
5.00 min

@Temperature 153 °C
5.00 min

@Temperature 307 °F
85.91% Gel content
5.00 min

@Temperature 155 °C
5.00 min

@Temperature 311 °F
88.68% Gel content
8.00 min

@Temperature 135 °C
8.00 min

@Temperature 275 °F
50.98% Gel content
8.00 min

@Temperature 138 °C
8.00 min

@Temperature 280 °F
64.91% Gel content
8.00 min

@Temperature 140 °C
8.00 min

@Temperature 284 °F
75.72% Gel content
8.00 min

@Temperature 143 °C
8.00 min

@Temperature 289 °F
82.31% Gel content
8.00 min

@Temperature 145 °C
8.00 min

@Temperature 293 °F
85.12% Gel content
8.00 min

@Temperature 148 °C
8.00 min

@Temperature 298 °F
87.17% Gel content
8.00 min

@Temperature 150 °C
8.00 min

@Temperature 302 °F
89.42% Gel content
8.00 min

@Temperature 153 °C
8.00 min

@Temperature 307 °F
88.74% Gel content
8.00 min

@Temperature 155 °C
8.00 min

@Temperature 311 °F
89.18% Gel content
10.0 min

@Temperature 150 °C
10.0 min

@Temperature 302 °F
89.38% Gel content
10.0 min

@Temperature 153 °C
10.0 min

@Temperature 307 °F
90.26% Gel content
10.0 min

@Temperature 155 °C
10.0 min

@Temperature 311 °F
89.93% Gel content
10.0 min

@Temperature 135 °C
10.0 min

@Temperature 275 °F
66.37% Gel content
10.0 min

@Temperature 138 °C
10.0 min

@Temperature 280 °F
77.72% Gel content
10.0 min

@Temperature 140 °C
10.0 min

@Temperature 284 °F
81.8% Gel content
10.0 min

@Temperature 143 °C
10.0 min

@Temperature 289 °F
84.41% Gel content
10.0 min

@Temperature 145 °C
10.0 min

@Temperature 293 °F
87.77% Gel content
10.0 min

@Temperature 148 °C
10.0 min

@Temperature 298 °F
88.48% Gel content
13.0 min

@Temperature 135 °C
13.0 min

@Temperature 275 °F
75.71% Gel content
13.0 min

@Temperature 138 °C
13.0 min

@Temperature 280 °F
79.7% Gel content
13.0 min

@Temperature 140 °C
13.0 min

@Temperature 284 °F
84.53% Gel content
13.0 min

@Temperature 143 °C
13.0 min

@Temperature 289 °F
86.24% Gel content
13.0 min

@Temperature 145 °C
13.0 min

@Temperature 293 °F
86.85% Gel content
13.0 min

@Temperature 148 °C
13.0 min

@Temperature 298 °F
88.92% Gel content
13.0 min

@Temperature 150 °C
13.0 min

@Temperature 302 °F
88.91% Gel content
13.0 min

@Temperature 153 °C
13.0 min

@Temperature 307 °F
89.95% Gel content
13.0 min

@Temperature 155 °C
13.0 min

@Temperature 311 °F
89.9% Gel content
15.0 min

@Temperature 135 °C
15.0 min

@Temperature 275 °F
79.98% Gel content
15.0 min

@Temperature 138 °C
15.0 min

@Temperature 280 °F
83.72% Gel content
15.0 min

@Temperature 140 °C
15.0 min

@Temperature 284 °F
86.78% Gel content
15.0 min

@Temperature 143 °C
15.0 min

@Temperature 289 °F
87.12% Gel content
15.0 min

@Temperature 145 °C
15.0 min

@Temperature 293 °F
89.11% Gel content
15.0 min

@Temperature 148 °C
15.0 min

@Temperature 298 °F
89.94% Gel content
15.0 min

@Temperature 150 °C
15.0 min

@Temperature 302 °F
89.6% Gel content
15.0 min

@Temperature 153 °C
15.0 min

@Temperature 307 °F
89.41% Gel content
15.0 min

@Temperature 155 °C
15.0 min

@Temperature 311 °F
90.16% Gel content
18.0 min

@Temperature 135 °C
18.0 min

@Temperature 275 °F
82.27% Gel content
18.0 min

@Temperature 138 °C
18.0 min

@Temperature 280 °F
85.13% Gel content
18.0 min

@Temperature 140 °C
18.0 min

@Temperature 284 °F
86.94% Gel content
18.0 min

@Temperature 143 °C
18.0 min

@Temperature 289 °F
89.65% Gel content
Users viewing this material also viewed the following: