Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

LyondellBasell Hifaxâ„¢ CB228 Thermoplastic Olefin Resin

Category Polymer , Thermoplastic
Manufacturer LyondellBasell
Trade Name Hifax™
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF LyondellBasell Hifaxâ„¢ CB228 Thermoplastic Olefin Resin.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
Key Features: medium melt flow, medium high modulus, paintable thermoplastic elastomeric olefin resin, excellent impact and stiffness balance, good paintability, good processabilityApplications: automotive claddings and rocker panelsDescription: Hifax CB228 medium melt flow, mineral-filled thermoplastic elastomeric olefin resin has an excelent combination of stiffness and dynamic impact characteristics. It was designed primarily for automotive exterior ornamentation applications.Information provided by Montell Polyolefins.LyondellBasell is the successor company to Montell.
Physical Properties Metric English Comments
Density 0.990 g/cc
0.0358 lb/in³
ISO 1183
Linear Mold Shrinkage 0.0090 cm/cm
0.0090 in/in
Tool, Montell
Melt Flow 8.0 g/10 min

@Load 2.16 kg,
Temperature 230 °C
8.0 g/10 min

@Load 4.76 lb,
Temperature 446 °F
ASTM D1238
Mechanical Properties Metric English Comments
Tensile Strength, Yield 20.0 MPa
2900 psi
ISO R527-1
Elongation at Yield 10 %
10 %
ISO R527-1
Flexural Modulus 1.30 GPa
189 ksi
ISO 178
Izod Impact, Notched 0.350 J/cm

@Temperature -40.0 °C
0.656 ft-lb/in

@Temperature -40.0 °F
ISO 180
Impact Test 23.0 J

@Temperature -30.0 °C
17.0 ft-lb

@Temperature -22.0 °F
MAII, E at Max Load, Ductile; ISO 6603-2
Thermal Properties Metric English Comments
CTE, linear 62.0 µm/m-°C

@Temperature -30.0 - 100 °C
34.4 µin/in-°F

@Temperature -22.0 - 212 °F
ASTM D696
Deflection Temperature at 0.46 MPa (66 psi) 83.0 °C
181 °F
ISO 75
Deflection Temperature at 1.8 MPa (264 psi) 46.0 °C
115 °F
ISO 75
Users viewing this material also viewed the following:
Copyright © lookpolymers.com All Rights Reserved