Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Multibase SILASTIC® C7-4535 TBPB Dow-Corning Biomedical Grade ETR Elastomer

Category Polymer , Thermoplastic , Elastomer, TPE , Silicone, Thermoplastic
Manufacturer Multibase
Trade Name SILASTIC®
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Multibase SILASTIC® C7-4535 TBPB Dow-Corning Biomedical Grade ETR Elastomer.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
Information provided by Multibase
Mechanical Properties Metric English Comments
Hardness, Shore A 34
34
as molded
37
37
post cured- 2 hours at 177°C
40
40
post cured- 4 hours at 204°C
Tensile Strength, Ultimate 7.72 MPa
1120 psi
post cured- 4 hours at 204°C
8.170 MPa
1185 psi
post cured- 2 hours at 177°C
8.62 MPa
1250 psi
as molded
Tensile Strength, Yield 1.07 MPa
155 psi
at 200%, as molded
1.48 MPa
215 psi
at 200%, post cured- 2 hours at 177°C
1.55 MPa
225 psi
200%, post cured- 4 hours at 204°C
Elongation at Break 727 %
727 %
post cured- 4 hours at 204°C
817 %
817 %
post cured- 2 hours at 177°C
958 %
958 %
as molded
Tear Strength 25.8 kN/m
147 pli
post cured- 4 hours at 204°C; Die B
26.1 kN/m
149 pli
post cured- 2 hours at 177°C; Die B
27.0 kN/m
154 pli
as molded; Die B
Copyright © lookpolymers.com All Rights Reserved