Overview of materials for Acrylonitrile Butadiene Styrene (ABS), 20% Glass Fiber Filled

Category Polymer , Thermoplastic , ABS Polymer , Acrylonitrile Butadiene Styrene (ABS), 20% Glass Fiber Filled
Manufacturer
Trade Name
Port Shanghai port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Overview of materials for Acrylonitrile Butadiene Styrene (ABS), 20% Glass Fiber Filled.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
This property data is a summary of similar materials in the MatWeb database for the category "Acrylonitrile Butadiene Styrene (ABS), 20% Glass Fiber Filled". Specific grades with glass content between 15% and 24% are included. Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.
Physical Properties Metric English Comments
Density 1.10 - 1.44 g/cc
0.0397 - 0.0520 lb/in³
Average value: 1.21 g/cc Grade Count:81
Filler Content 15.0 - 20.0 %
15.0 - 20.0 %
Average value: 18.4 % Grade Count:21
Water Absorption 0.130 - 1.00 %
0.130 - 1.00 %
Average value: 0.252 % Grade Count:29
Moisture Absorption at Equilibrium 0.200 %
0.200 %
Average value: 0.200 % Grade Count:4
Water Absorption at Saturation 0.300 - 1.00 %
0.300 - 1.00 %
Average value: 0.775 % Grade Count:4
Maximum Moisture Content 0.0200 - 0.150
0.0200 - 0.150
Average value: 0.0417 Grade Count:6
Linear Mold Shrinkage 0.00100 - 0.00900 cm/cm
0.00100 - 0.00900 in/in
Average value: 0.00256 cm/cm Grade Count:72
Linear Mold Shrinkage, Transverse 0.00200 - 0.00700 cm/cm
0.00200 - 0.00700 in/in
Average value: 0.00429 cm/cm Grade Count:7
Melt Flow 0.100 - 17.0 g/10 min
0.100 - 17.0 g/10 min
Average value: 6.10 g/10 min Grade Count:34
Ash 15.0 - 20.0 %
15.0 - 20.0 %
Average value: 19.0 % Grade Count:5
Mechanical Properties Metric English Comments
Hardness, Rockwell M 44.0 - 103
44.0 - 103
Average value: 78.7 Grade Count:6
Hardness, Rockwell R 87.0 - 124
87.0 - 124
Average value: 110 Grade Count:29
Tensile Strength, Ultimate 35.0 - 93.2 MPa
5080 - 13500 psi
Average value: 67.7 MPa Grade Count:49
8.00 - 60.0 MPa

@Temperature 60.0 - 90.0 °C
1160 - 8700 psi

@Temperature 140 - 194 °F
Average value: 29.6 MPa Grade Count:3
Tensile Strength, Yield 45.5 - 108 MPa
6600 - 15600 psi
Average value: 74.5 MPa Grade Count:40
Elongation at Break 1.00 - 11.0 %
1.00 - 11.0 %
Average value: 3.08 % Grade Count:67
1.50 - 15.0 %

@Temperature 60.0 - 90.0 °C
1.50 - 15.0 %

@Temperature 140 - 194 °F
Average value: 6.32 % Grade Count:2
Elongation at Yield 1.50 - 5.00 %
1.50 - 5.00 %
Average value: 3.00 % Grade Count:8
1.00 - 1.00 %

@Temperature 90.0 - 90.0 °C
1.00 - 1.00 %

@Temperature 194 - 194 °F
Average value: 1.00 % Grade Count:1
Modulus of Elasticity 3.50 - 12.2 GPa
508 - 1770 ksi
Average value: 5.54 GPa Grade Count:33
2.90 - 5.30 GPa

@Temperature 60.0 - 90.0 °C
421 - 769 ksi

@Temperature 140 - 194 °F
Average value: 4.05 GPa Grade Count:2
Flexural Yield Strength 65.5 - 142 MPa
9500 - 20600 psi
Average value: 104 MPa Grade Count:65
Flexural Modulus 2.50 - 6.86 GPa
363 - 996 ksi
Average value: 5.24 GPa Grade Count:71
2.10 - 2.10 GPa

@Temperature 60.0 - 60.0 °C
305 - 305 ksi

@Temperature 140 - 140 °F
Average value: 2.10 GPa Grade Count:1
Izod Impact, Notched 0.392 - 1.35 J/cm
0.735 - 2.54 ft-lb/in
Average value: 0.713 J/cm Grade Count:66
0.400 - 0.600 J/cm

@Temperature -40.0 - 0.000 °C
0.749 - 1.12 ft-lb/in

@Temperature -40.0 - 32.0 °F
Average value: 0.475 J/cm Grade Count:3
0.400 - 0.500 J/cm

@Temperature -30.0 - 0.000 °C
0.749 - 0.937 ft-lb/in

@Temperature -22.0 - 32.0 °F
Average value: 0.475 J/cm Grade Count:1
0.400 - 0.500 J/cm

@Thickness 3.20 - 3.20 mm
0.749 - 0.937 ft-lb/in

@Thickness 0.126 - 0.126 in
Average value: 0.475 J/cm Grade Count:1
Izod Impact, Unnotched 1.60 - 4.00 J/cm
3.00 - 7.50 ft-lb/in
Average value: 2.93 J/cm Grade Count:30
Izod Impact, Notched (ISO) 6.00 - 16.0 kJ/m²
2.86 - 7.61 ft-lb/in²
Average value: 8.14 kJ/m² Grade Count:7
5.00 - 6.00 kJ/m²

@Temperature -30.0 - -30.0 °C
2.38 - 2.86 ft-lb/in²

@Temperature -22.0 - -22.0 °F
Average value: 5.67 kJ/m² Grade Count:3
Izod Impact, Unnotched (ISO) 18.0 - 20.0 kJ/m²
8.57 - 9.52 ft-lb/in²
Average value: 19.3 kJ/m² Grade Count:3
15.0 - 15.0 kJ/m²

@Temperature -30.0 - -30.0 °C
7.14 - 7.14 ft-lb/in²

@Temperature -22.0 - -22.0 °F
Average value: 15.0 kJ/m² Grade Count:1
Charpy Impact Unnotched 0.800 - 30.0 J/cm²
3.81 - 143 ft-lb/in²
Average value: 6.23 J/cm² Grade Count:6
0.400 - 5.00 J/cm²

@Temperature -40.0 - -20.0 °C
1.90 - 23.8 ft-lb/in²

@Temperature -40.0 - -4.00 °F
Average value: 2.36 J/cm² Grade Count:4
Charpy Impact, Notched 0.200 - 0.700 J/cm²
0.952 - 3.33 ft-lb/in²
Average value: 0.529 J/cm² Grade Count:12
0.200 - 0.600 J/cm²

@Temperature -30.0 - -20.0 °C
0.952 - 2.86 ft-lb/in²

@Temperature -22.0 - -4.00 °F
Average value: 0.450 J/cm² Grade Count:6
Thermal Properties Metric English Comments
CTE, linear 21.0 - 54.0 µm/m-°C
11.7 - 30.0 µin/in-°F
Average value: 36.5 µm/m-°C Grade Count:18
Melting Point 165 - 225 °C
329 - 437 °F
Average value: 205 °C Grade Count:3
Maximum Service Temperature, Air 60.0 - 75.0 °C
140 - 167 °F
Average value: 66.3 °C Grade Count:4
Hot Ball Pressure Test 80.0 - 100 °C
176 - 212 °F
Average value: 94.5 °C Grade Count:4
Deflection Temperature at 0.46 MPa (66 psi) 82.0 - 195 °C
180 - 383 °F
Average value: 107 °C Grade Count:46
Deflection Temperature at 1.8 MPa (264 psi) 71.0 - 175 °C
160 - 347 °F
Average value: 100 °C Grade Count:67
Vicat Softening Point 85.0 - 117 °C
185 - 243 °F
Average value: 104 °C Grade Count:25
UL RTI, Electrical 50.0 - 60.0 °C
122 - 140 °F
Average value: 55.7 °C Grade Count:6
UL RTI, Mechanical with Impact 50.0 - 60.0 °C
122 - 140 °F
Average value: 55.7 °C Grade Count:6
Electrical Properties Metric English Comments
Electrical Resistivity 500000 - 1.00e+16 ohm-cm
500000 - 1.00e+16 ohm-cm
Average value: 2.88e+15 ohm-cm Grade Count:33
Surface Resistance 1e+05 - 1.00e+15 ohm
1e+05 - 1.00e+15 ohm
Average value: 1.50e+14 ohm Grade Count:16
Static Decay 2.00 sec
2.00 sec
Average value: 2.00 sec Grade Count:5
Dielectric Constant 2.60 - 3.50
2.60 - 3.50
Average value: 3.03 Grade Count:8
Dielectric Strength 15.7 - 35.0 kV/mm
400 - 889 kV/in
Average value: 21.3 kV/mm Grade Count:25
Dissipation Factor 0.00400 - 0.0200
0.00400 - 0.0200
Average value: 0.00830 Grade Count:7
Arc Resistance 80.0 - 180 sec
80.0 - 180 sec
Average value: 103 sec Grade Count:3
Comparative Tracking Index 250 - 600 V
250 - 600 V
Average value: 502 V Grade Count:11