Material Notes:
This property data is a summary of similar materials in the MatWeb database for the category "ECTFE Fluoropolymer". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.
Physical Properties Metric English Comments
Density 1.18 - 1.87 g/cc
0.0426 - 0.0676 lb/in³
Average value: 1.67 g/cc Grade Count:34
Water Absorption 0.0100 - 0.100 %
0.0100 - 0.100 %
Average value: 0.0550 % Grade Count:8
Water Absorption at Saturation 0.100 %
0.100 %
Average value: 0.100 % Grade Count:14
Linear Mold Shrinkage 0.00200 - 0.0250 cm/cm
0.00200 - 0.0250 in/in
Average value: 0.0232 cm/cm Grade Count:13
Melt Flow 1.00 - 550 g/10 min
1.00 - 550 g/10 min
Average value: 31.9 g/10 min Grade Count:22
Mechanical Properties Metric English Comments
Hardness, Rockwell R 73.0 - 120
73.0 - 120
Average value: 90.8 Grade Count:16
Hardness, Shore D 69.0 - 85.0
69.0 - 85.0
Average value: 75.2 Grade Count:17
Tensile Strength, Ultimate 19.0 - 55.0 MPa
2760 - 7980 psi
Average value: 47.8 MPa Grade Count:18
Tensile Strength, Yield 29.0 - 68.9 MPa
4210 - 10000 psi
Average value: 32.2 MPa Grade Count:17
Elongation at Break 1.00 - 300 %
1.00 - 300 %
Average value: 222 % Grade Count:20
Elongation at Yield 1.00 - 10.0 %
1.00 - 10.0 %
Average value: 5.04 % Grade Count:14
Modulus of Elasticity 1.20 - 1.96 GPa
174 - 284 ksi
Average value: 1.67 GPa Grade Count:19
Flexural Yield Strength 26.2 - 114 MPa
3800 - 16500 psi
Average value: 49.8 MPa Grade Count:17
Flexural Modulus 1.65 - 6.21 GPa
240 - 900 ksi
Average value: 1.94 GPa Grade Count:18
Izod Impact, Notched 0.250 J/cm - NB
0.468 ft-lb/in - NB
Average value: 2.26 J/cm Grade Count:17
0.640 - 1.22 J/cm

@Temperature -40.0 - -40.0 °C
1.20 - 2.29 ft-lb/in

@Temperature -40.0 - -40.0 °F
Average value: 1.86 J/cm Grade Count:2
0.190 - 2.10 J/cm

@Temperature -40.0 - -40.0 °C
0.356 - 3.93 ft-lb/in

@Temperature -40.0 - -40.0 °F
Average value: 1.86 J/cm Grade Count:12
0.190 - 2.10 J/cm

@Thickness 3.20 - 3.20 mm
0.356 - 3.93 ft-lb/in

@Thickness 0.126 - 0.126 in
Average value: 1.86 J/cm Grade Count:12
Coefficient of Friction 0.190 - 0.860
0.190 - 0.860
Average value: 0.252 Grade Count:18
Coefficient of Friction, Static 0.190 - 0.300
0.190 - 0.300
Average value: 0.279 Grade Count:15
Taber Abrasion, mg/1000 Cycles 5.00
5.00
Average value: 5.00 Grade Count:15
Thermal Properties Metric English Comments
CTE, linear 18.0 - 101 µm/m-°C
10.0 - 56.0 µin/in-°F
Average value: 91.5 µm/m-°C Grade Count:19
135 - 135 µm/m-°C

@Temperature 85.0 - 125 °C
75.0 - 75.0 µin/in-°F

@Temperature 185 - 257 °F
Average value: 135 µm/m-°C Grade Count:2
Specific Heat Capacity 0.946 - 0.962 J/g-°C
0.226 - 0.230 BTU/lb-°F
Average value: 0.960 J/g-°C Grade Count:15
Thermal Conductivity 0.150 - 0.231 W/m-K
1.04 - 1.60 BTU-in/hr-ft²-°F
Average value: 0.167 W/m-K Grade Count:5
0.150 - 0.150 W/m-K

@Temperature 40.0 - 40.0 °C
1.04 - 1.04 BTU-in/hr-ft²-°F

@Temperature 104 - 104 °F
Average value: 0.150 W/m-K Grade Count:13
Melting Point 220 - 242 °C
428 - 468 °F
Average value: 237 °C Grade Count:31
Crystallization Temperature 205 - 222 °C
401 - 432 °F
Average value: 221 °C Grade Count:13
Maximum Service Temperature, Air 140 - 150 °C
284 - 302 °F
Average value: 148 °C Grade Count:7
Deflection Temperature at 0.46 MPa (66 psi) 90.0 - 232 °C
194 - 450 °F
Average value: 100 °C Grade Count:17
Deflection Temperature at 1.8 MPa (264 psi) 62.8 - 210 °C
145 - 410 °F
Average value: 72.8 °C Grade Count:19
Brittleness Temperature -76.0 - 20.0 °C
-105 - 68.0 °F
Average value: -69.6 °C Grade Count:15
Glass Transition Temp, Tg 85.0 °C
185 °F
Average value: 85.0 °C Grade Count:13
Flammability, UL94 V-0
V-0
Grade Count:20
Oxygen Index 52.0 - 60.0 %
52.0 - 60.0 %
Average value: 53.1 % Grade Count:19
Electrical Properties Metric English Comments
Electrical Resistivity 1.00e+15 - 1.00e+17 ohm-cm
1.00e+15 - 1.00e+17 ohm-cm
Average value: 4.71e+16 ohm-cm Grade Count:18
Surface Resistance 1.00e+12 - 1.00e+17 ohm
1.00e+12 - 1.00e+17 ohm
Average value: 5.25e+16 ohm Grade Count:4
Dielectric Constant 2.47 - 2.60
2.47 - 2.60
Average value: 2.55 Grade Count:19
Dielectric Strength 13.8 - 105 kV/mm
350 - 2670 kV/in
Average value: 28.7 kV/mm Grade Count:20
Dissipation Factor 0.00120 - 0.0140
0.00120 - 0.0140
Average value: 0.00525 Grade Count:4
Comparative Tracking Index 600 V
600 V
Average value: 600 V Grade Count:3