Material Notes:
This property data is a summary of similar materials in the MatWeb database for the category "Phenolic, Novolac, Mineral/Fiber Filled". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.
Physical Properties Metric English Comments
Density 1.46 - 1.58 g/cc
0.0527 - 0.0571 lb/in³
Average value: 1.50 g/cc Grade Count:10
Apparent Bulk Density 0.500 - 0.680 g/cc
0.0181 - 0.0246 lb/in³
Average value: 0.586 g/cc Grade Count:10
Water Absorption 0.300 - 0.400 %
0.300 - 0.400 %
Average value: 0.360 % Grade Count:10
Linear Mold Shrinkage 0.00400 - 0.0110 cm/cm
0.00400 - 0.0110 in/in
Average value: 0.00760 cm/cm Grade Count:10
Mechanical Properties Metric English Comments
Tensile Strength, Ultimate 41.0 - 62.0 MPa
5950 - 8990 psi
Average value: 53.6 MPa Grade Count:10
Modulus of Elasticity 9.00 - 11.0 GPa
1310 - 1600 ksi
Average value: 10.1 GPa Grade Count:6
Flexural Yield Strength 72.0 - 86.0 MPa
10400 - 12500 psi
Average value: 81.1 MPa Grade Count:10
Flexural Modulus 6.90 GPa
1000 ksi
Average value: 6.90 GPa Grade Count:4
Compressive Yield Strength 166 - 235 MPa
24100 - 34100 psi
Average value: 197 MPa Grade Count:10
Izod Impact, Notched 0.210 - 0.290 J/cm
0.393 - 0.543 ft-lb/in
Average value: 0.250 J/cm Grade Count:4
Thermal Properties Metric English Comments
Maximum Service Temperature, Air 150 - 160 °C
302 - 320 °F
Average value: 157 °C Grade Count:6
Deflection Temperature at 1.8 MPa (264 psi) 177 - 191 °C
351 - 376 °F
Average value: 186 °C Grade Count:6
UL RTI, Electrical 150 °C
302 °F
Average value: 150 °C Grade Count:4
UL RTI, Mechanical with Impact 150 °C
302 °F
Average value: 150 °C Grade Count:4
UL RTI, Mechanical without Impact 150 °C
302 °F
Average value: 150 °C Grade Count:4
Flammability, UL94 V-1 - V-0
V-1 - V-0
Grade Count:10
Electrical Properties Metric English Comments
Electrical Resistivity 2.20e+10 - 1.00e+12 ohm-cm
2.20e+10 - 1.00e+12 ohm-cm
Average value: 7.55e+11 ohm-cm Grade Count:8
Dielectric Constant 5.00 - 5.50
5.00 - 5.50
Average value: 5.13 Grade Count:6
Dielectric Strength 10.8 - 14.7 kV/mm
274 - 373 kV/in
Average value: 12.5 kV/mm Grade Count:10
Dissipation Factor 0.0400 - 0.0500
0.0400 - 0.0500
Average value: 0.0483 Grade Count:6
Comparative Tracking Index 180 - 225 V
180 - 225 V
Average value: 191 V Grade Count:10