Overview of materials for Polybutylene Terephthalate (PBT), 10% Glass Fiber Filled

Category Polymer , Thermoplastic , Polyester, TP , Polybutylene Terephthalate (PBT) , Polybutylene Terephthalate (PBT), 10% Glass Fiber Filled
Manufacturer
Trade Name
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Overview of materials for Polybutylene Terephthalate (PBT), 10% Glass Fiber Filled.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
This property data is a summary of similar materials in the MatWeb database for the category "Polybutylene Terephthalate (PBT), 10% Glass Fiber Filled".Specific grades with glass content between 5% and 14% are included. Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.
Physical Properties Metric English Comments
Density 1.11 - 1.55 g/cc
0.0401 - 0.0560 lb/in³
Average value: 1.39 g/cc Grade Count:88
1.19 - 1.31 g/cc

@Temperature 250 - 250 °C
0.0430 - 0.0473 lb/in³

@Temperature 482 - 482 °F
Average value: 1.25 g/cc Grade Count:2
Filler Content 5.00 - 15.0 %
5.00 - 15.0 %
Average value: 10.0 % Grade Count:13
Water Absorption 0.0600 - 0.500 %
0.0600 - 0.500 %
Average value: 0.273 % Grade Count:25
Moisture Absorption at Equilibrium 0.0400 - 0.220 %
0.0400 - 0.220 %
Average value: 0.155 % Grade Count:31
Viscosity 240000 - 240000 cP

@Temperature 250 - 250 °C
240000 - 240000 cP

@Temperature 482 - 482 °F
Average value: 240000 cP Grade Count:1
240000 - 240000 cP

@Shear Rate 1000 - 1000 1/s
240000 - 240000 cP

@Shear Rate 1000 - 1000 1/s
Average value: 240000 cP Grade Count:1
Viscosity Test 80.0 - 145 cm³/g
80.0 - 145 cm³/g
Average value: 110 cm³/g Grade Count:7
Maximum Moisture Content 0.0200
0.0200
Average value: 0.0200 Grade Count:6
Linear Mold Shrinkage 0.00100 - 0.0200 cm/cm
0.00100 - 0.0200 in/in
Average value: 0.00804 cm/cm Grade Count:75
Linear Mold Shrinkage, Transverse 0.00100 - 0.0160 cm/cm
0.00100 - 0.0160 in/in
Average value: 0.00953 cm/cm Grade Count:32
Melt Flow 4.00 - 60.0 g/10 min
4.00 - 60.0 g/10 min
Average value: 23.0 g/10 min Grade Count:41
Mechanical Properties Metric English Comments
Hardness, Rockwell M 83.0 - 120
83.0 - 120
Average value: 98.2 Grade Count:6
Hardness, Rockwell R 117 - 119
117 - 119
Average value: 118 Grade Count:7
Ball Indentation Hardness 160 - 170 MPa
23200 - 24700 psi
Average value: 163 MPa Grade Count:3
Tensile Strength, Ultimate 12.5 - 110 MPa
1810 - 16000 psi
Average value: 75.0 MPa Grade Count:65
50.0 - 130 MPa

@Temperature -20.0 - 100 °C
7250 - 18900 psi

@Temperature -4.00 - 212 °F
Average value: 53.1 MPa Grade Count:1
3.73 - 125 MPa

@Temperature -40.0 - 160 °C
541 - 18100 psi

@Temperature -40.0 - 320 °F
Average value: 53.1 MPa Grade Count:2
3.73 - 125 MPa

@Strain 0.250 - 10.0 %
541 - 18100 psi

@Strain 0.250 - 10.0 %
Average value: 53.1 MPa Grade Count:2
Tensile Strength, Yield 49.0 - 100 MPa
7100 - 14500 psi
Average value: 76.6 MPa Grade Count:32
Elongation at Break 2.50 - 100 %
2.50 - 100 %
Average value: 7.61 % Grade Count:71
Elongation at Yield 3.50 - 4.00 %
3.50 - 4.00 %
Average value: 3.80 % Grade Count:4
Modulus of Elasticity 2.80 - 6.20 GPa
406 - 899 ksi
Average value: 4.54 GPa Grade Count:54
Flexural Yield Strength 75.0 - 165 MPa
10900 - 23900 psi
Average value: 121 MPa Grade Count:63
50.0 - 50.0 MPa

@Temperature 90.0 - 90.0 °C
7250 - 7250 psi

@Temperature 194 - 194 °F
Average value: 50.0 MPa Grade Count:1
Flexural Modulus 0.373 - 9.00 GPa
54.0 - 1310 ksi
Average value: 4.01 GPa Grade Count:61
Shear Modulus >= 0.219 GPa

@Temperature -50.0 - 200 °C
>= 31.8 ksi

@Temperature -58.0 - 392 °F
Average value: 0.780 GPa Grade Count:2
Secant Modulus 1.04857 - 6.80 GPa

@Temperature -40.0 - 100 °C
152.085 - 986 ksi

@Temperature -40.0 - 212 °F
Average value: 3.63 GPa Grade Count:1
1.04857 - 6.80 GPa

@Strain 0.250 - 3.50 %
152.085 - 986 ksi

@Strain 0.250 - 3.50 %
Average value: 3.63 GPa Grade Count:1
Izod Impact, Notched 0.267 - 1.60 J/cm
0.500 - 3.00 ft-lb/in
Average value: 0.570 J/cm Grade Count:31
0.48051 - 0.48051 J/cm

@Temperature -28.9 - -28.9 °C
0.90019 - 0.90019 ft-lb/in

@Temperature -20.0 - -20.0 °F
Average value: 0.481 J/cm Grade Count:1
Izod Impact, Unnotched 3.20 - 9.61 J/cm
6.00 - 18.0 ft-lb/in
Average value: 5.96 J/cm Grade Count:8
Izod Impact, Notched (ISO) 3.80 - 23.0 kJ/m²
1.81 - 10.9 ft-lb/in²
Average value: 6.79 kJ/m² Grade Count:17
3.00 - 5.00 kJ/m²

@Temperature -30.0 - -30.0 °C
1.43 - 2.38 ft-lb/in²

@Temperature -22.0 - -22.0 °F
Average value: 4.33 kJ/m² Grade Count:3
Izod Impact, Unnotched (ISO) 23.0 - 45.0 kJ/m²
10.9 - 21.4 ft-lb/in²
Average value: 36.5 kJ/m² Grade Count:11
26.0 - 40.0 kJ/m²

@Temperature -30.0 - -30.0 °C
12.4 - 19.0 ft-lb/in²

@Temperature -22.0 - -22.0 °F
Average value: 33.0 kJ/m² Grade Count:2
Charpy Impact Unnotched 2.00 J/cm² - NB
9.52 ft-lb/in² - NB
Average value: 3.95 J/cm² Grade Count:44
2.00 - 19.0 J/cm²

@Temperature -30.0 - 30.0 °C
9.52 - 90.4 ft-lb/in²

@Temperature -22.0 - 86.0 °F
Average value: 4.92 J/cm² Grade Count:32
Charpy Impact, Notched 0.230 - 1.80 J/cm²
1.09 - 8.57 ft-lb/in²
Average value: 0.703 J/cm² Grade Count:50
0.210 - 1.00 J/cm²

@Temperature -30.0 - 30.0 °C
0.999 - 4.76 ft-lb/in²

@Temperature -22.0 - 86.0 °F
Average value: 0.582 J/cm² Grade Count:31
Puncture Energy 1.50 - 1.50 J

@Temperature -30.0 - -30.0 °C
1.11 - 1.11 ft-lb

@Temperature -22.0 - -22.0 °F
Average value: 1.50 J Grade Count:1
Tensile Creep Modulus, 1 hour 3000 - 5500 MPa
435000 - 798000 psi
Average value: 4530 MPa Grade Count:6
Tensile Creep Modulus, 1000 hours 2000 - 5000 MPa
290000 - 725000 psi
Average value: 3580 MPa Grade Count:6
Electrical Properties Metric English Comments
Electrical Resistivity 1.00e+6 - 1.00e+17 ohm-cm
1.00e+6 - 1.00e+17 ohm-cm
Average value: 9.89e+15 ohm-cm Grade Count:55
Surface Resistance 1.00e+6 - 1.00e+17 ohm
1.00e+6 - 1.00e+17 ohm
Average value: 7.79e+15 ohm Grade Count:36
Dielectric Constant 3.00 - 4.30
3.00 - 4.30
Average value: 3.56 Grade Count:34
Dielectric Strength 18.5 - 100 kV/mm
470 - 2540 kV/in
Average value: 26.3 kV/mm Grade Count:49
Dissipation Factor 0.00100 - 0.0600
0.00100 - 0.0600
Average value: 0.0116 Grade Count:25
Dielectric Loss Index 0.00200 - 0.0200
0.00200 - 0.0200
Average value: 0.0170 Grade Count:6
Arc Resistance 60.0 - 180 sec
60.0 - 180 sec
Average value: 117 sec Grade Count:14
Comparative Tracking Index 125 - 600 V
125 - 600 V
Average value: 287 V Grade Count:39
Hot Wire Ignition, HWI 7.00 - 120 sec
7.00 - 120 sec
Average value: 25.9 sec Grade Count:6
Users viewing this material also viewed the following: