Material Notes:
This property data is a summary of similar materials in the MatWeb database for the category "Polyphthalamide". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.
Physical Properties Metric English Comments
Density 1.10 - 3.80 g/cc
0.0397 - 0.137 lb/in³
Average value: 1.49 g/cc Grade Count:605
1.10 - 1.10 g/cc

@Temperature 325 - 325 °C
0.0397 - 0.0397 lb/in³

@Temperature 617 - 617 °F
Average value: 1.10 g/cc Grade Count:1
Filler Content 3.00 - 65.0 %
3.00 - 65.0 %
Average value: 33.1 % Grade Count:234
Water Absorption 0.0200 - 10.0 %
0.0200 - 10.0 %
Average value: 0.410 % Grade Count:239
0.850 - 1.35 %

@Temperature 70.0 - 70.0 °C
0.850 - 1.35 %

@Temperature 158 - 158 °F
Average value: 1.09 % Grade Count:16
Moisture Absorption at Equilibrium 0.100 - 2.40 %
0.100 - 2.40 %
Average value: 0.507 % Grade Count:80
Additive Loading 4.00 - 50.0 %
4.00 - 50.0 %
Average value: 32.1 % Grade Count:16
Linear Mold Shrinkage 0.000 - 0.0250 cm/cm
0.000 - 0.0250 in/in
Average value: 0.00452 cm/cm Grade Count:531
Linear Mold Shrinkage, Transverse 0.000800 - 0.105 cm/cm
0.000800 - 0.105 in/in
Average value: 0.00839 cm/cm Grade Count:221
Melt Flow 5.00 - 50.0 g/10 min
5.00 - 50.0 g/10 min
Average value: 20.0 g/10 min Grade Count:6
Spiral Flow 30.0 - 70.0 cm
11.8 - 27.6 in
Average value: 47.7 cm Grade Count:6
Mechanical Properties Metric English Comments
Hardness, Rockwell M 105 - 109
105 - 109
Average value: 107 Grade Count:3
Hardness, Rockwell R 110 - 127
110 - 127
Average value: 124 Grade Count:87
Ball Indentation Hardness 270 - 360 MPa
39200 - 52200 psi
Average value: 320 MPa Grade Count:11
Tensile Strength, Ultimate 6.13 - 385 MPa
889 - 55800 psi
Average value: 171 MPa Grade Count:557
24.1 - 265 MPa

@Temperature -40.0 - 230 °C
3500 - 38400 psi

@Temperature -40.0 - 446 °F
Average value: 84.7 MPa Grade Count:31
100 - 145 MPa

@Temperature 130 - 180 °C
14500 - 21000 psi

@Temperature 266 - 356 °F
Average value: 84.7 MPa Grade Count:13
100 - 145 MPa

@Time 1.80e+7 - 7.20e+7 sec
14500 - 21000 psi

@Time 5000 - 20000 hour
Average value: 84.7 MPa Grade Count:13
3.94 - 321.27 MPa

@Strain 0.0400 - 5.10 %
571 - 46596 psi

@Strain 0.0400 - 5.10 %
Average value: 84.7 MPa Grade Count:6
3.94 - 321.27 MPa

@Temperature -40.0 - 180 °C
571 - 46596 psi

@Temperature -40.0 - 356 °F
Average value: 84.7 MPa Grade Count:6
Tensile Strength, Yield 12.0 - 307 MPa
1740 - 44500 psi
Average value: 154 MPa Grade Count:81
20.0 - 119 MPa

@Temperature 100 - 175 °C
2900 - 17300 psi

@Temperature 212 - 347 °F
Average value: 64.8 MPa Grade Count:8
Elongation at Break 0.563 - 100 %
0.563 - 100 %
Average value: 2.83 % Grade Count:548
1.00 - 95.0 %

@Temperature -40.0 - 230 °C
1.00 - 95.0 %

@Temperature -40.0 - 446 °F
Average value: 6.00 % Grade Count:36
Elongation at Yield 0.700 - 50.0 %
0.700 - 50.0 %
Average value: 3.09 % Grade Count:86
3.10 - 10.0 %

@Temperature 100 - 150 °C
3.10 - 10.0 %

@Temperature 212 - 302 °F
Average value: 4.92 % Grade Count:4
Modulus of Elasticity 1.70 - 48.3 GPa
247 - 7000 ksi
Average value: 13.9 GPa Grade Count:561
0.500 - 32.0 GPa

@Temperature -40.0 - 230 °C
72.5 - 4640 ksi

@Temperature -40.0 - 446 °F
Average value: 8.06 GPa Grade Count:40
Flexural Yield Strength 58.8 - 530 MPa
8530 - 76900 psi
Average value: 261 MPa Grade Count:531
9.00 - 352 MPa

@Temperature -40.0 - 200 °C
1310 - 51100 psi

@Temperature -40.0 - 392 °F
Average value: 119 MPa Grade Count:22
96.0 - 181 MPa

@Temperature 100 - 200 °C
13900 - 26300 psi

@Temperature 212 - 392 °F
Average value: 119 MPa Grade Count:2
96.0 - 181 MPa

@Strain 3.50 - 5.00 %
13900 - 26300 psi

@Strain 3.50 - 5.00 %
Average value: 119 MPa Grade Count:2
Flexural Modulus 1.79 - 41.4 GPa
260 - 6000 ksi
Average value: 12.3 GPa Grade Count:549
0.400 - 16.8 GPa

@Temperature -40.0 - 200 °C
58.0 - 2440 ksi

@Temperature -40.0 - 392 °F
Average value: 5.22 GPa Grade Count:23
Compressive Yield Strength 100 - 314 MPa
14500 - 45500 psi
Average value: 186 MPa Grade Count:33
71.0 - 355 MPa

@Temperature -40.0 - 200 °C
10300 - 51500 psi

@Temperature -40.0 - 392 °F
Average value: 171 MPa Grade Count:1
Poissons Ratio 0.290 - 0.410
0.290 - 0.410
Average value: 0.383 Grade Count:32
Shear Modulus 0.852 - 6.74 GPa
124 - 978 ksi
Average value: 3.53 GPa Grade Count:15
0.0768 - 4.00 GPa

@Temperature -50.0 - 350 °C
11.1 - 580 ksi

@Temperature -58.0 - 662 °F
Average value: 2.35 GPa Grade Count:5
Shear Strength 44.1 - 108 MPa
6400 - 15700 psi
Average value: 79.2 MPa Grade Count:53
Secant Modulus 1.70799 - 14.8867 GPa

@Temperature 0.000 - 200 °C
247.727 - 2159.17 ksi

@Temperature 32.0 - 392 °F
Average value: 10.1 GPa Grade Count:1
1.70799 - 14.8867 GPa

@Strain 0.0500 - 4.13 %
247.727 - 2159.17 ksi

@Strain 0.0500 - 4.13 %
Average value: 10.1 GPa Grade Count:1
Izod Impact, Notched 0.147 - 11.0 J/cm
0.276 - 20.6 ft-lb/in
Average value: 1.12 J/cm Grade Count:380
0.910 - 7.50 J/cm

@Temperature -40.0 - -40.0 °C
1.70 - 14.1 ft-lb/in

@Temperature -40.0 - -40.0 °F
Average value: 2.61 J/cm Grade Count:3
Izod Impact, Unnotched 0.801 - 5340 J/cm
1.50 - 10000 ft-lb/in
Average value: 6.47 J/cm Grade Count:296
Izod Impact, Notched (ISO) 2.00 - 115 kJ/m²
0.952 - 54.7 ft-lb/in²
Average value: 14.7 kJ/m² Grade Count:182
3.00 - 75.0 kJ/m²

@Temperature -40.0 - -20.0 °C
1.43 - 35.7 ft-lb/in²

@Temperature -40.0 - -4.00 °F
Average value: 14.8 kJ/m² Grade Count:22
Izod Impact, Unnotched (ISO) 12.0 kJ/m² - NB
5.71 ft-lb/in² - NB
Average value: 53.1 kJ/m² Grade Count:124
23.0 kJ/m² - NB

@Temperature -40.0 - -5.00 °C
10.9 ft-lb/in² - NB

@Temperature -40.0 - 23.0 °F
Average value: 45.5 kJ/m² Grade Count:5
Charpy Impact Unnotched 0.473 J/cm² - NB
2.25 ft-lb/in² - NB
Average value: 5.66 J/cm² Grade Count:158
1.20 - 999.9 J/cm²

@Temperature -40.0 - -20.0 °C
5.71 - 4759 ft-lb/in²

@Temperature -40.0 - -4.00 °F
Average value: 4.71 J/cm² Grade Count:44
Charpy Impact, Notched 0.100 J/cm² - NB
0.476 ft-lb/in² - NB
Average value: 1.18 J/cm² Grade Count:147