Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Plenco 4414 Phenolic, Granular, Transfer Molded

Category Polymer , Thermoset , Filled/Reinforced Thermoset , Phenolic , Phenolic, Novolac, Mineral/Flock Filled
Manufacturer Plenco (Plastics Engineering Company)
Trade Name
Port Shanghai port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Plenco 4414 Phenolic, Granular, Transfer Molded.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
PLENCO 04414 is a flock and mineral filled phenolic molding compound. It is formulated for use in electrical applications that require improved heat resistance, mechanical strength, and dimensional stability. UL recognized under component file E40654. 04414 is available in black.Information supplied by Plenco.
Physical Properties Metric English Comments
Bulk Density 0.630 g/cc
0.0228 lb/in³
ASTM D1895
Density 1.54 g/cc
0.0556 lb/in³
ASTM D792
Water Absorption 0.21 %
0.21 %
ASTM D570
Linear Mold Shrinkage 0.0034 cm/cm
0.0034 in/in
ASTM D955
Mechanical Properties Metric English Comments
Hardness, Rockwell E 79
79
ASTM D785
Tensile Strength, Ultimate 52.0 MPa
7540 psi
ASTM D638
Elongation at Break 0.61 %
0.61 %
ASTM D638
Tensile Modulus 10.1 GPa
1460 ksi
ASTM D638
Flexural Strength 94.0 MPa
13600 psi
ASTM D790
Flexural Modulus 9.50 GPa
1380 ksi
ASTM D790
Compressive Strength 175 MPa
25400 psi
ASTM D695
Izod Impact, Notched 0.236 J/cm
0.442 ft-lb/in
ASTM D256
Charpy Impact, Notched 0.218 J/cm²
1.04 ft-lb/in²
ASTM D256
Impact 113
113
J/m Drop Ball Impact; PLENCO
Thermal Properties Metric English Comments
Maximum Service Temperature, Air 203 °C
397 °F
Heat Resistance; ASTM D570D
Deflection Temperature at 1.8 MPa (264 psi) 195 °C
383 °F
ASTM D648
Flammability, UL94 V-1

@Thickness 1.50 mm
V-1

@Thickness 0.0591 in
Oxygen Index 31 %
31 %
ASTM D2863
Shrinkage 0.145 %
0.145 %
72 hr, 120ºC; ASTM D1299
Electrical Properties Metric English Comments
Volume Resistivity 4.10e+11 ohm-cm
4.10e+11 ohm-cm
ASTM D247
Dielectric Constant 5.3
5.3
ASTM D150
Dielectric Strength 11.9 kV/mm
302 kV/in
Short Time; ASTM D149
Dissipation Factor 0.051
0.051
ASTM D150
Arc Resistance 162 sec
162 sec
ASTM D495
Comparative Tracking Index 175 V
175 V
ASTM D3638