Plenco 4548 Phenolic, Granular, Transfer Molded

Category Polymer , Thermoset , Filled/Reinforced Thermoset , Phenolic , Phenolic, Novolac, Mineral Filled
Manufacturer Plenco (Plastics Engineering Company)
Trade Name
Port Shanghai port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Plenco 4548 Phenolic, Granular, Transfer Molded.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
PLENCO 04548 is a heat resistant mineral filled phenolic molding compound, offering fast cure rates and hot rigidity. Type ASTM 5948 CFG, and UL recognized under component file E40654. 04548 is available in black and brown.Information supplied by Plenco.
Physical Properties Metric English Comments
Bulk Density 0.690 g/cc
0.0249 lb/in³
ASTM D1895
Density 1.47 g/cc
0.0531 lb/in³
ASTM D792
Water Absorption 0.215 %
0.215 %
ASTM D570
Linear Mold Shrinkage 0.0052 cm/cm
0.0052 in/in
ASTM D955
Mechanical Properties Metric English Comments
Hardness, Rockwell E 87
87
ASTM D785
Tensile Strength, Ultimate 60.0 MPa
8700 psi
ASTM D638
Elongation at Break 0.80 %
0.80 %
ASTM D638
Tensile Modulus 9.00 GPa
1310 ksi
ASTM D638
Flexural Strength 98.0 MPa
14200 psi
ASTM D790
Flexural Modulus 9.00 GPa
1310 ksi
ASTM D790
Compressive Strength 208 MPa
30200 psi
ASTM D695
Poissons Ratio 0.34
0.34
ASTM D638
Shear Modulus 3.36 GPa
487 ksi
Calculated
Izod Impact, Notched 0.171 J/cm
0.320 ft-lb/in
ASTM D256
Charpy Impact, Notched 0.200 J/cm²
0.952 ft-lb/in²
ASTM D256
Impact 104
104
J/m Drop Ball Impact; PLENCO
Thermal Properties Metric English Comments
CTE, linear 65.0 µm/m-°C

@Temperature 40.0 - 130 °C
36.1 µin/in-°F

@Temperature 104 - 266 °F
TMA; ASTM E831
Thermal Conductivity 0.440 W/m-K

@Temperature 100 °C
3.05 BTU-in/hr-ft²-°F

@Temperature 212 °F
ASTM E1461
Maximum Service Temperature, Air 204 °C
399 °F
Heat Resistance; ASTM D570D
Deflection Temperature at 1.8 MPa (264 psi) 189 °C
372 °F
ASTM D648
Flammability, UL94 V-0

@Thickness 1.50 mm
V-0

@Thickness 0.0591 in
Oxygen Index 27.3 %
27.3 %
ASTM D2863
Shrinkage 0.199 %
0.199 %
72 hr, 120ºC; ASTM D1299
Electrical Properties Metric English Comments
Volume Resistivity 7.10e+11 ohm-cm
7.10e+11 ohm-cm
ASTM D247
Dielectric Constant 5.3
5.3
ASTM D150
Dielectric Strength 12.3 kV/mm
312 kV/in
Short Time; ASTM D149
Dissipation Factor 0.056
0.056
ASTM D150
Arc Resistance 144 sec
144 sec
ASTM D495
Comparative Tracking Index 175 V
175 V
ASTM D3638