Material Notes:
Quadrant Engineering Plastic Products is marketing non-UV-stabilized polycarbonate stock shapes under the trade name Quadrant PC 1000. It is a natural, “non-optical” industrial quality (clear, translucent). High mechanical strength Good creep resistance Very high impact strength, even at low temperatures Stiffness retention over a wide range of temperatures Very good dimensional stability (very low water absorption and low coefficient of linear thermal expansion) Natural colour (clear, translucent) Good electrical insulating and dielectric properties Physiologically inert (suitable for food contact) Economical thermal performance
Physical Properties Metric English Comments
Density 1.20 g/cc
0.0434 lb/in³
ISO 1183-1
Moisture Absorption at Equilibrium 0.15 %
0.15 %
50% RH
Water Absorption at Saturation 0.40 %
0.40 %
Mechanical Properties Metric English Comments
Hardness, Rockwell M 75
75
ISO 2039-2
Hardness, Shore D 79
79
Ball Indentation Hardness 120 MPa
17400 psi
ISO 2039-1
Tensile Strength 74.0 MPa
10700 psi
at Yield; ISO 527-1/-2
Elongation at Break >= 50 %
>= 50 %
ISO 527-1/-2
Elongation at Yield 6.0 %
6.0 %
ISO 527-1/-2
Tensile Modulus 2.40 GPa
348 ksi
ISO 527-1/-2
Flexural Strength 103 MPa
14900 psi
Flexural Modulus 2.175 GPa
315.5 ksi
Compressive Strength 21.0 MPa

@Strain 1 %
3050 psi

@Strain 1 %
ISO 604
40.0 MPa

@Strain 2 %
5800 psi

@Strain 2 %
ISO 604
80.0 MPa

@Strain 5 %
11600 psi

@Strain 5 %
ISO 604
K Factor (ISO) 60 µm/km
60 µm/km
Charpy Impact Unnotched NB
NB
ISO 179-1/1eU
Charpy Impact, Notched 0.900 J/cm²
4.28 ft-lb/in²
ISO 179-1/1eA
Coefficient of Friction, Dynamic 0.50 - 0.60
0.50 - 0.60
Thermal Properties Metric English Comments
CTE, linear 65.0 µm/m-°C

@Temperature 23.0 - 100 °C
36.1 µin/in-°F

@Temperature 73.4 - 212 °F
Thermal Conductivity 0.210 W/m-K
1.46 BTU-in/hr-ft²-°F
Maximum Service Temperature, Air 120 °C
248 °F
Continuous; 20,000 h
130 °C
266 °F
Continuous; 5,000 h
Deflection Temperature at 1.8 MPa (264 psi) 130 °C
266 °F
ISO 75-1/-2
Glass Transition Temp, Tg 150 °C
302 °F
DSC, 20°C/min.; ISO 11357-1/-2
Flammability, UL94 HB
HB
Oxygen Index 25 %
25 %
ISO 4589-1/-2
Electrical Properties Metric English Comments
Volume Resistivity >= 1.0e+14 ohm-cm
>= 1.0e+14 ohm-cm
IEC 60093
Surface Resistivity per Square >= 1.0e+13 ohm
>= 1.0e+13 ohm
IEC 60093
Dielectric Constant 3.0

@Frequency >=100000 Hz
3.0

@Frequency >=100000 Hz
IEC 60250
Dielectric Strength 28.0 kV/mm
711 kV/in
Dissipation Factor 0.0010

@Frequency 100000 Hz
0.0010

@Frequency 100000 Hz
IEC 60250
Comparative Tracking Index 350 V
350 V
IEC 60112
Compliance Properties Metric English Comments
3A-Dairy No
No
European Food 1935/2004 No
No
FDA Yes
Yes
USP Class VI No
No
Chemical Resistance Properties Metric English Comments
Acids, Strong (pH 1-3) Unacceptable
Unacceptable
Acids, Weak Limited
Limited
Alcohols Limited
Limited
Alkalies, Strong (pH 11-14) Unacceptable
Unacceptable
Alkalies, Weak Limited
Limited
Chlorinated Solvents Unacceptable
Unacceptable
Continuous Sunlight Limited
Limited
Hot Water / Steam Limited
Limited
Hydrocarbons - Aliphatic Acceptable
Acceptable
Hydrocarbons - Aromatic Unacceptable
Unacceptable
Inorganic Salt Solutions Acceptable
Acceptable
Ketones, Esters Unacceptable
Unacceptable
Users viewing this material also viewed the following:
Copyright © lookpolymers.com All Rights Reserved