Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

SABIC Innovative Plastics Geloy XP4034 ASA (Europe-Africa-Middle East)

Category Polymer , Thermoplastic , ASA Polymer , Polycarbonate (PC) , Polycarbonate/ASA Alloy, Unreinforced
Manufacturer SABIC Innovative Plastics (GE Plastics)
Trade Name GELOY
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF SABIC Innovative Plastics Geloy XP4034 ASA (Europe-Africa-Middle East).pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
GELOY XP4034 is a high heat modified ASA+PC alloy. It is a weatherable, injection mouldable product which is available in a wide range of colours. The product is recommended for automotive unpainted exterior applications.This data was supplied by SABIC-IP for the Europe-Africa-Middle East region.
Physical Properties Metric English Comments
Density 1.15 g/cc
0.0415 lb/in³
ISO 1183
Moisture Absorption at Equilibrium 0.25 %
0.25 %
23°C / 50% RH; ISO 62
Water Absorption at Saturation 0.70 %

@Temperature 23.0 °C
0.70 %

@Temperature 73.4 °F
ISO 62
Linear Mold Shrinkage, Flow 0.0040 - 0.0060 cm/cm
0.0040 - 0.0060 in/in
on tensile bar; SABIC Method
Melt Flow 15 g/10 min

@Load 5.00 kg,
Temperature 260 °C
15 g/10 min

@Load 11.0 lb,
Temperature 500 °F
[cm^3/10 min] Melt Volume Rate; ISO 1133
Mechanical Properties Metric English Comments
Hardness, H358/30 98.0 MPa
14200 psi
ISO 2039-1
Tensile Strength at Break 45.0 MPa
6530 psi
50 mm/min; ISO 527
Tensile Strength, Yield 55.0 MPa
7980 psi
50 mm/min; ISO 527
Elongation at Break 35 %
35 %
50 mm/min; ISO 527
Elongation at Yield 4.5 %
4.5 %
50 mm/min; ISO 527
Tensile Modulus 2.35 GPa
341 ksi
1 mm/min; ISO 527
Flexural Yield Strength 85.0 MPa
12300 psi
2 mm/min; ISO 178
Flexural Modulus 2.50 GPa
363 ksi
2 mm/min; ISO 178
Izod Impact, Notched (ISO) 8.00 kJ/m²

@Temperature -30.0 °C
3.81 ft-lb/in²

@Temperature -22.0 °F
80*10*4; ISO 180/1A
33.0 kJ/m²

@Temperature 23.0 °C
15.7 ft-lb/in²

@Temperature 73.4 °F
80*10*4; ISO 180/1A
Taber Abrasion, mg/1000 Cycles 120

@Load 1.00 kg
120

@Load 2.20 lb
CS-17; SABIC Method
Thermal Properties Metric English Comments
Deflection Temperature at 0.46 MPa (66 psi) 112 °C
234 °F
Edgew 120*10*4 sp=100mm; ISO 75/Be
Deflection Temperature at 1.8 MPa (264 psi) 100 °C
212 °F
Edgew 120*10*4 sp=100mm; ISO 75/Ae
Vicat Softening Point 107 °C
225 °F
Rate B/50; ISO 306
109 °C
228 °F
Rate B/120; ISO 306