Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

SABIC Innovative Plastics LNP LUBRILOY R2000 PA 66 (Asia Pacific)

Category Polymer , Thermoplastic , Nylon , Nylon 66
Manufacturer SABIC Innovative Plastics (GE Plastics)
Trade Name LNP Lubriloy
Port Shanghai port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF SABIC Innovative Plastics LNP LUBRILOY R2000 PA 66 (Asia Pacific).pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
LNP* Lubriloy* R2000 is a compound based on Nylon 66 resin containing Proprietary Lubricant. Added features of this material include: Internally Lubricated.
Physical Properties Metric English Comments
Density 1.03 g/cc
0.0372 lb/in³
ASTM D792
1.03 g/cc
0.0372 lb/in³
ISO 1183
Moisture Absorption 0.250 %
0.250 %
50% RH, 24 hrs; ASTM D570
Linear Mold Shrinkage, Flow 0.018 - 0.022 cm/cm

@Time 86400 sec
0.018 - 0.022 in/in

@Time 24.0 hour
ASTM D955
Linear Mold Shrinkage, Transverse 0.021 - 0.031 cm/cm

@Time 86400 sec
0.021 - 0.031 in/in

@Time 24.0 hour
ASTM D955
Mechanical Properties Metric English Comments
Tensile Strength at Break 53.0 MPa
7690 psi
ISO 527
55.0 MPa
7980 psi
ASTM D638
Tensile Strength, Yield 56.0 MPa
8120 psi
ASTM D638
Elongation at Break 27 %
27 %
ASTM D638
32.3 %
32.3 %
ISO 527
Elongation at Yield 14 %
14 %
ASTM D638
Tensile Modulus 2.41 GPa
350 ksi
50 mm/min; ASTM D638
Flexural Strength 65.0 MPa
9430 psi
ISO 178
82.0 MPa
11900 psi
ASTM D790
Flexural Modulus 2.00 GPa
290 ksi
ISO 178
2.31 GPa
335 ksi
ASTM D790
Izod Impact, Notched 0.620 J/cm
1.16 ft-lb/in
ASTM D256
Izod Impact, Unnotched 17.24 J/cm
32.30 ft-lb/in
ASTM D4812
Izod Impact, Notched (ISO) 6.00 kJ/m²
2.86 ft-lb/in²
80*10*4; ISO 180/1A
Izod Impact, Unnotched (ISO) 141 kJ/m²
67.1 ft-lb/in²
80*10*4; ISO 180/1U
Coefficient of Friction, Dynamic 0.36
0.36
ASTM D3702 Modified
Coefficient of Friction, Static 0.27
0.27
ASTM D3702 Modified
K (wear) Factor 101 x 10-8 mm³/N-M
50.0 x 10-10 in³-min/ft-lb-hr
Washer; ASTM D3702 Modified
Thermal Properties Metric English Comments
CTE, linear, Parallel to Flow 77.4 µm/m-°C

@Temperature -40.0 - 40.0 °C
43.0 µin/in-°F

@Temperature -40.0 - 104 °F
ASTM E 831
CTE, linear, Transverse to Flow 103 µm/m-°C

@Temperature -40.0 - 40.0 °C
57.2 µin/in-°F

@Temperature -40.0 - 104 °F
ASTM E 831
Deflection Temperature at 1.8 MPa (264 psi) 85.0 °C
185 °F
Flatw 80*10*4 sp=64mm; ISO 75/Af
77.0 °C

@Thickness 3.20 mm
171 °F

@Thickness 0.126 in
unannealed; ASTM D648
Users viewing this material also viewed the following: