SABIC Innovative Plastics Valox® V8030CS PBT+PET

Category Polymer , Thermoplastic , Polyester, TP , Polybutylene Terephthalate (PBT) , PBT + PET Blend, Glass Filled , Polyethylene Terephthalate (PET)
Manufacturer SABIC Innovative Plastics (GE Plastics)
Trade Name Valox®
Port Shanghai port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF SABIC Innovative Plastics Valox® V8030CS PBT+PET.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
Glass filled Valox with enhanced surface
Physical Properties Metric English Comments
Density 1.43 g/cc
0.0517 lb/in³
ASTM D792
1.43 g/cc
0.0517 lb/in³
ISO 1183
Melt Index of Compound 16 g/10 min

@Load 2.16 kg,
Temperature 265 °C
16 g/10 min

@Load 4.76 lb,
Temperature 509 °F
MVR [cm^3/10 min]; ISO 1133
42 g/10 min

@Load 5.00 kg,
Temperature 265 °C
42 g/10 min

@Load 11.0 lb,
Temperature 509 °F
MVR [cm^3/10 min]; ISO 1133
Mechanical Properties Metric English Comments
Tensile Strength at Break 92.0 MPa
13300 psi
5 mm/min; ISO 527
98.0 MPa
14200 psi
Type I, 5 mm/min; ASTM D638
Tensile Strength, Yield 95.0 MPa
13800 psi
5 mm/min; ISO 527
99.0 MPa
14400 psi
Type I, 5 mm/min; ASTM D638
Elongation at Break 2.0 %
2.0 %
5 mm/min; ISO 527
2.8 %
2.8 %
Type I, 5 mm/min; ASTM D638
3.4 %
3.4 %
Flexural Strain, break, 2 mm/min; ISO 178
8.6 %
8.6 %
Nominal Strain, 5 mm/min; ASTM D638
Elongation at Yield 2.1 %
2.1 %
5 mm/min; ISO 527
2.7 %
2.7 %
Type I, 5 mm/min; ASTM D638
Tensile Modulus 5.69 GPa
825 ksi
5 mm/min; ASTM D638
5.88 GPa
853 ksi
1 mm/min; ISO 527
Flexural Strength 148 MPa
21500 psi
ISO 178
151 MPa
21900 psi
1.3 mm/min, 50 mm span; ASTM D790
Flexural Yield Strength 151 MPa
21900 psi
1.3 mm/min, 50 mm span; ASTM D790
Flexural Modulus 5.38 GPa
780 ksi
1.3 mm/min, 50 mm span; ASTM D790
5.48 GPa
795 ksi
ISO 178
Izod Impact, Notched 0.580 J/cm
1.09 ft-lb/in
ASTM D256
Izod Impact, Notched (ISO) 4.00 kJ/m²
1.90 ft-lb/in²
80*10*4; ISO 180/1A
4.00 kJ/m²

@Temperature -30.0 °C
1.90 ft-lb/in²

@Temperature -22.0 °F
80*10*4; ISO 180/1A
Charpy Impact, Notched 2.30 J/cm²
10.9 ft-lb/in²
80*10*4mm, Cut; ISO 179/1eA
Thermal Properties Metric English Comments
Deflection Temperature at 0.46 MPa (66 psi) 216 °C

@Thickness 3.20 mm
421 °F

@Thickness 0.126 in
ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 88.0 °C

@Thickness 3.20 mm
190 °F

@Thickness 0.126 in
ASTM D648
Vicat Softening Point 222 °C
432 °F
Rate A/50; ISO 306
222 °C
432 °F
Rate A/120; ISO 306
224 °C
435 °F
Rate A/50; ASTM D1525