Category Ceramic , Oxide , Silicon Oxide
Manufacturer Skamol Group
Trade Name Moler
Port Shanghai port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Skamol Group Moler BB-Filler Aggregate Insulation.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
SKAMOL insulating aggregates have the following characteristics: Max. service temperature: Up to 900°C (1652°F)Back-up insulationLightweightGood insulating propertiesChemically inertDue to free-flowing properties Moler aggregates are ideally suitable as a loose-fill insulation for furnace cavities and double skin linings, over arched roofs and in open joints, leveling of furnace bottoms and hearths.Information provided by Skamol.
Physical Properties Metric English Comments
Bulk Density 0.545 g/cc
0.0197 lb/in³
As Supplied
Loss On Ignition 1.50 %

@Temperature 1025 °C
1.50 %

@Temperature 1877 °F
Thermal Properties Metric English Comments
Thermal Conductivity 0.160 W/m-K

@Temperature 200 °C
1.11 BTU-in/hr-ft²-°F

@Temperature 392 °F
Mean temp.; BS 1902 Section 5.5 1991
0.180 W/m-K

@Temperature 400 °C
1.25 BTU-in/hr-ft²-°F

@Temperature 752 °F
BS 1902 Section 5.5 1991
0.200 W/m-K

@Temperature 600 °C
1.39 BTU-in/hr-ft²-°F

@Temperature 1110 °F
BS 1902 Section 5.5 1991
Maximum Service Temperature, Air 900 °C
1650 °F
Component Elements Properties Metric English Comments
Al2O3 9.0 %
9.0 %
CaO 0.80 %
0.80 %
Fe2O3 7.0 %
7.0 %
K2O 1.6 %
1.6 %
MgO 1.3 %
1.3 %
Na2O 0.40 %
0.40 %
SiO2 77 %
77 %
SO3 1.2 %
1.2 %
TiO2 0.70 %
0.70 %
Descriptive Properties Value Comments
Color Red-Brown
Pyrometric Cone Equivalent 1350°C
ASTM C24-89, ORTON cones