Material Notes:
A nickel-chromium-iron-molybdenum alloy with outstanding strength and oxidation resistance at temperatures to 2200°F (1200°C). Matrix stiffening provided by the molybdenum content results in high strength in a solid-solution alloy having good fabrication characteristics. Used in gas turbines, industrial furnaces, heat-treating equipment, and nuclear engineering. Standard product forms are round, extruded section, flats, forging stock, plate, sheet, strip, and wire.Data provided by the manufacturer, Special Metals.
Physical Properties Metric English Comments
Density 8.23 g/cc
0.297 lb/in³
Mechanical Properties Metric English Comments
Tensile Strength, Ultimate 630 MPa

@Temperature 550 °C
91400 psi

@Temperature 1020 °F
Solution Annealed prior to test
825 MPa

@Temperature 23.0 °C
120000 psi

@Temperature 73.4 °F
Tensile Strength, Yield 375 MPa

@Strain 0.200 %
54400 psi

@Strain 0.200 %
Solution Annealed. Value at room temperature
210 MPa

@Strain 0.200 %,
Temperature 550 °C
30500 psi

@Strain 0.200 %,
Temperature 1020 °F
Solution Annealed prior to test
Elongation at Break 42 %
42 %
Solution Annealed
48 %

@Temperature 550 °C
48 %

@Temperature 1020 °F
Solution Annealed prior to test.
Thermal Properties Metric English Comments
CTE, linear 13.3 µm/m-°C

@Temperature 20.0 - 100 °C
7.39 µin/in-°F

@Temperature 68.0 - 212 °F
Specific Heat Capacity 0.461 J/g-°C
0.110 BTU/lb-°F
Thermal Conductivity 11.6 W/m-K
80.5 BTU-in/hr-ft²-°F
Melting Point 1260 - 1355 °C
2300 - 2471 °F
Solidus 1260 °C
2300 °F
Liquidus 1355 °C
2471 °F
Component Elements Properties Metric English Comments
Carbon, C 0.50 - 2.5 %
0.50 - 2.5 %
Chromium, Cr 20.5 - 23 %
20.5 - 23 %
Cobalt, Co 0.50 - 2.5 %
0.50 - 2.5 %
Iron, Fe 17 - 20 %
17 - 20 %
Manganese, Mn <= 1.0 %
<= 1.0 %
Molybdenum, Mo 8.0 - 10 %
8.0 - 10 %
Nickel, Ni 45 %
45 %
As remainder
Phosphorous, P <= 0.040 %
<= 0.040 %
Silicon, Si <= 1.0 %
<= 1.0 %
Sulfur, S <= 0.030 %
<= 0.030 %
Tungsten, W 0.20 - 1.0 %
0.20 - 1.0 %
Electrical Properties Metric English Comments
Electrical Resistivity 0.000116 ohm-cm
0.000116 ohm-cm
Magnetic Permeability 1.011
1.011
at 200 oersted (15.9 kA/m)