Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Specialty Coating Systems Parylene N Poly (P-Xylylene) Coating

Category Polymer , Film , Thermoplastic , Poly (P-Xylylene)
Manufacturer Specialty Coating Systems (SCS)
Trade Name Parylene
Port Shanghai port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Specialty Coating Systems Parylene N Poly (P-Xylylene) Coating.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
Parylene N, poly(para-xylylene), is a completely linear, highly crystalline material. Parylene N is a primary dielectric, exhibiting a very low dissipation factor, high dielectric strength, and a low dielectric constant invariant with frequency. The crevice-penetrating ability of Parylene N is second only to that of Parylene HT®.SCS Parylene conformal coatings are ultra-thin, pinhole-free polymer coatings that provide a number of high-value surface treatment properties such as excellent moisture, chemical and dielectric barrier properties, thermal and UV stability, and dry-film lubricity. Parylene coatings are used in a number of applications throughout the medical device, electronics, automotive, military and aerospace industries.Information provided by Specialty Coating Systems (SCS) .
Physical Properties Metric English Comments
Water Vapor Permeability 0.590 g mil/ (m2 day)

@Temperature 37.0 °C
0.0381 g mil/ (100 in2 day)

@Temperature 98.6 °F
90% RH; ASTM E96
Density 1.10 - 1.12 g/cc
0.0397 - 0.0405 lb/in³
ASTM D1505
Water Absorption <= 0.10 %

@Time 86400 sec
<= 0.10 %

@Time 24.0 hour
ASTM D570
Oxygen Transmission 15.4 cc-mm/m²-24hr-atm

@Temperature 25.0 °C
39.1 cc-mil/100 in²-24hr-atm

@Temperature 77.0 °F
ASTM D1434
Nitrogen Transmission 3.00 cc-mm/m²-24hr-atm

@Temperature 25.0 °C
7.62 cc-mil/100 in²-24hr-atm

@Temperature 77.0 °F
ASTM D1434
Carbon Dioxide Transmission 84.3 cc-mm/m²-24hr-atm

@Temperature 25.0 °C
214 cc-mil/100 in²-24hr-atm

@Temperature 77.0 °F
ASTM D1434
Mechanical Properties Metric English Comments
Hardness, Rockwell R 85
85
ASTM D785
Tensile Strength 48.3 MPa
7000 psi
Tensile Strength, Yield 42.1 MPa
6100 psi
ASTM D882
Elongation at Break <= 250 %
<= 250 %
ASTM D882
Elongation at Yield 2.5 %
2.5 %
ASTM D882
Modulus of Elasticity 2.41 GPa
350 ksi
Secant; ASTM D882
Coefficient of Friction, Dynamic 0.25
0.25
ASTM D1894
Coefficient of Friction, Static 0.25
0.25
ASTM D1894
Thermal Properties Metric English Comments
CTE, linear 69.0 µm/m-°C
38.3 µin/in-°F
via TMA
Specific Heat Capacity 0.837 J/g-°C
0.200 BTU/lb-°F
Thermal Conductivity 0.126 W/m-K
0.874 BTU-in/hr-ft²-°F
ASTM C177
Melting Point 420 °C
788 °F
via DSC
Maximum Service Temperature, Air 60.0 °C
140 °F
Continuous
80.0 °C
176 °F
Short Term
Softening Point 160 °C
320 °F
T5 Point - modulus = 690 MPa (100,000 psi)
>= 300 °C
>= 572 °F
T4 point - modulus = 70 MPa (10,000 psi)
Optical Properties Metric English Comments
Refractive Index 1.661
1.661
n<sub>D</sub>; Abbe Refractometer
Transmission, Visible 80 %

@Wavelength 400 nm
80 %

@Wavelength 400 nm
UV Transmittance <= 1.0 %

@Wavelength 277 nm
<= 1.0 %

@Wavelength 277 nm
cutoff
60 %

@Wavelength 300 nm
60 %

@Wavelength 300 nm
75 %

@Wavelength 350 nm
75 %

@Wavelength 350 nm
Electrical Properties Metric English Comments
Volume Resistivity 1.40e+17 ohm-cm
1.40e+17 ohm-cm
50% RH; ASTM D257
Surface Resistance 1.00e+13 ohm
1.00e+13 ohm
50% RH; ASTM D257
Dielectric Constant 2.65

@Frequency 60.0 Hz
2.65

@Frequency 60.0 Hz
ASTM D150
2.65

@Frequency 1000 Hz
2.65

@Frequency 1000 Hz
ASTM D150
2.65

@Frequency 1.00e+6 Hz
2.65

@Frequency 1.00e+6 Hz
ASTM D150
Dielectric Strength 276 kV/mm
7000 kV/in
ASTM D149
Dissipation Factor 0.00020

@Frequency 60.0 Hz
0.00020

@Frequency 60.0 Hz
ASTM D150
0.00020

@Frequency 1000 Hz
0.00020

@Frequency 1000 Hz
ASTM D150
0.00060

@Frequency 1.00e+6 Hz
0.00060

@Frequency 1.00e+6 Hz
ASTM D150
Compliance Properties Metric English Comments
USP Class VI Yes
Yes
Descriptive Properties Value Comments
Biocompatibility ISO 10993
Hydrogen Transmission 212.6 cc-mm/m²-24hr-atm
ASTM D1434
UV Stability > 2000 hours
ASTM G154
Users viewing this material also viewed the following:
Copyright © lookpolymers.com All Rights Reserved