Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

TSE Industries Millathane® 76 Millable Polyester Polyurethane Rubber, 0.75 PHR Zinc Stearate

Category Polymer , Thermoset , Polyester, TS , Polyurethane, TS , Thermoset Polyurethane, Elastomer, Unreinforced , Rubber or Thermoset Elastomer (TSE)
Manufacturer TSE Industries, Inc
Trade Name Millathane®
Port Shanghai port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF TSE Industries Millathane® 76 Millable Polyester Polyurethane Rubber, 0.75 PHR Zinc Stearate.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
Millathane® 76 is a very suitable choice for use in products such as bushings, small copier rolls; automotive applications — bumpers, o-rings, hydraulic seals, belts, gaskets, solid tires — and many other high performance polyurethane applications. Millathane 76 can be vulcanized by sulfur or peroxide cured systems.Zinc stearate has replaced cadmium stearate due to toxicity concerns with cadmium compounds. Used as a coactivator with Thanecure® ZM it shortens cure times and improves compression set. Zinc stearate also functions as a process aid and release agent, and helps prevent sticking to mill or internal mixer surfaces.All information provided by TSE Industries
Mechanical Properties Metric English Comments
Hardness, Shore A 71
71
Tensile Strength, Yield 32.62 MPa
4731 psi
Elongation at Yield 559 %
559 %
100% Modulus 0.00361 GPa
0.524 ksi
200% Modulus 0.008143 GPa
1.181 ksi
300% Modulus 0.01427 GPa
2.069 ksi
Tear Strength 65.1 kN/m
371 pli
Die C
Compression Set 31.4 %

@Temperature 70.0 °C,
Time 79200 sec
31.4 %

@Temperature 158 °F,
Time 22.0 hour
Processing Properties Metric English Comments
Cure Time 8.00 min

@Temperature 155 °C
0.133 hour

@Temperature 311 °F
TC90