Material Notes:
This Material Specification applies to quenched and tempered heavy plates made of the special structural steel N-A-XTRA® This steel can be supplied with a minimum yield strength of 800 MPa. It can be delivered in two qualities with different toughness properties. 1) Quality for low service temperature with minimum impact energy at - 40 °C (N-A-XTRA® M) in a thickness range from 3 to 100 mm. 2) Special quality for low service temperature with minimum impact energy at - 60 °C (classic N-A-XTRA®) in a thickness range from 3 to 50 mm.Application: The steels are used for welded constructions of all kinds, such as pressure vessels, penstocks, bridges and structures, as well as transport vehicles, mobile cranes, mining equipment, hoistings and earth moving equipment, which are utilized in different types of climatic conditions.If continuous yielding occurs, the yield strength is determined as Rp0,2Information Provided by Thyssen Krupp
Mechanical Properties Metric English Comments
Tensile Strength at Break 840 - 990 MPa

@Thickness >=65.0 mm
122000 - 144000 psi

@Thickness >=2.56 in
840 - 1000 MPa

@Thickness 65.0 mm
122000 - 145000 psi

@Thickness 2.56 in
Tensile Strength, Yield >= 740 MPa

@Thickness >=65.0 mm
>= 107000 psi

@Thickness >=2.56 in
>= 800 MPa

@Thickness 65.0 mm
>= 116000 psi

@Thickness 2.56 in
Elongation at Break >= 11 %
>= 11 %
Charpy Impact 27.0 J

@Temperature -60.0 °C
19.9 ft-lb

@Temperature -76.0 °F
Transverse
30.0 J

@Temperature -40.0 °C
22.1 ft-lb

@Temperature -40.0 °F
Transverse
30.0 J

@Temperature -60.0 °C
22.1 ft-lb

@Temperature -76.0 °F
Longitudinal
35.0 J

@Temperature -20.0 °C
25.8 ft-lb

@Temperature -4.00 °F
Transverse
40.0 J

@Temperature -40.0 °C
29.5 ft-lb

@Temperature -40.0 °F
Longitudinal
40.0 J

@Temperature 0.000 °C
29.5 ft-lb

@Temperature 32.0 °F
Transverse
50.0 J

@Temperature -20.0 °C
36.9 ft-lb

@Temperature -4.00 °F
Longitudinal
60.0 J

@Temperature 0.000 °C
44.3 ft-lb

@Temperature 32.0 °F
Longitudinal
Component Elements Properties Metric English Comments
Aluminum, Al <= 1.5 %
<= 1.5 %
Carbon, C <= 0.20 %
<= 0.20 %
Chromium, Cr <= 1.5 %
<= 1.5 %
Manganese, Mn <= 1.6 %
<= 1.6 %
Molybdenum, Mo <= 0.60 %
<= 0.60 %
Phosphorous, P <= 0.20 %
<= 0.20 %
Silicon, Si <= 0.80 %
<= 0.80 %
Sulfur, S <= 0.010 %
<= 0.010 %