| Thermal Properties | Metric | English | Comments |
|---|---|---|---|
| CTE, linear, Parallel to Flow |
80.0
µm/m-°C <br>@Temperature 23.0 - 60.0 °C
|
44.4
µin/in-°F <br>@Temperature 73.4 - 140 °F
|
ISO 11359-2 |
|
SABIC Innovative Plastics Cycolac® G151 ABS (Europe-Africa-Middle East)
CYCOLAC G151 is a flame retardant grade of ´new technology´ CYCOLAC which has been especially formulated to minimise many of the problems often associated with the processing of traditiona..
|
|||
| CTE, linear, Parallel to Flow |
80.0
µm/m-°C <br>@Temperature 23.0 - 60.0 °C
|
44.4
µin/in-°F <br>@Temperature 73.4 - 140 °F
|
ISO 11359-2 |
|
SABIC Innovative Plastics Cycolac® S701SU ABS (Europe-Africa-Middle East)
CYCOLAC S701SU is an ABS with improved UV resistance, providing a superior balance of properties. Its wide processing window, excellent flow and good mechanical properties give this material an exce..
|
|||
| CTE, linear, Parallel to Flow |
80.0
µm/m-°C <br>@Temperature 23.0 - 60.0 °C
|
44.4
µin/in-°F <br>@Temperature 73.4 - 140 °F
|
ISO 11359-2 |
|
SABIC Innovative Plastics Cycolac® X37 ABS (Europe-Africa-Middle East)
CYCOLAC X37 is the highest heat material available in the CYCOLAC range of materials and is widely recognized within the automotive industry as being the industry standard for high heat ABS. It comb..
|
|||
| CTE, linear, Parallel to Flow |
80.0
µm/m-°C <br>@Temperature -40.0 - 40.0 °C
|
44.4
µin/in-°F <br>@Temperature -40.0 - 104 °F
|
ISO 11359-2 |
|
SABIC Innovative Plastics Cycoloy® FXC810FE PC+ABS (Europe-Africa-Middle East)
CYCOLOY FXC810FE is a multi-purpose PC+ABS injection moulding grade, suitable for those applications that require Ferrite colour effects. The colour package may effect performance.This data was supp..
|
|||
| CTE, linear, Parallel to Flow |
80.0
µm/m-°C <br>@Temperature 23.0 - 60.0 °C
|
44.4
µin/in-°F <br>@Temperature 73.4 - 140 °F
|
ISO 11359-2 |
|
SABIC Innovative Plastics Cycoloy® FXC813SK PC+ABS (Europe-Africa-Middle East)
CYCOLOY FXC813SK is a multi purpose PC+ABS injection moulding grade, providing a favourable balance of engineering properties. CYCOLOY FXC813SK is suitable for those applications that require sparkl..
|
|||
| CTE, linear, Parallel to Flow |
80.0
µm/m-°C <br>@Temperature 23.0 - 60.0 °C
|
44.4
µin/in-°F <br>@Temperature 73.4 - 140 °F
|
ISO 11359-2 |
|
SABIC Innovative Plastics GELOY HRA150 ASA (Europe-Africa-Middle East)
GELOY HRA150 is a high heat resistant ASA+PC. GELOY HRA150 shows high impact retention and color stability upon weathering, and hence can be positioned in various outdoor and indoor applications req..
|
|||
| CTE, linear, Parallel to Flow |
80.0
µm/m-°C <br>@Temperature 23.0 - 60.0 °C
|
44.4
µin/in-°F <br>@Temperature 73.4 - 140 °F
|
ISO 11359-2 |
|
SABIC Innovative Plastics LNP COLORCOMP AX98567H ABS
LNP* COLORCOMP* AX98567H is an unfilled compound based on ABS. Added feature of this grade is: Healthcare.
|
|||
| CTE, linear, Parallel to Flow |
80.0
µm/m-°C <br>@Temperature 20.0 °C
|
44.4
µin/in-°F <br>@Temperature 68.0 °F
|
ISO 11359-1/-2 |
|
DSM Arnite® D00 301 PET (European Grade)
(discontinued **)
Arnite resins are engineered to provide specific performance in applications where DSM technology can offer value.Arnite Molding resins: Standard Unfilled and Reinforced materialsHigh modulus Flame ..
|
|||
| CTE, linear, Parallel to Flow |
80.0
µm/m-°C <br>@Temperature 20.0 °C
|
44.4
µin/in-°F <br>@Temperature 68.0 °F
|
ISO 11359-1/-2 |
|
DSM Arnite® D04 300 PET (European Grade)
(discontinued **)
Arnite resins are engineered to provide specific performance in applications where DSM technology can offer value.Arnite Molding resins: Standard Unfilled and Reinforced materialsHigh modulus Flame ..
|
|||
| CTE, linear, Parallel to Flow |
80.0
µm/m-°C <br>@Temperature -40.0 - 40.0 °C
|
44.4
µin/in-°F <br>@Temperature -40.0 - 104 °F
|
ISO 11359-2 |
|
SABIC Innovative Plastics Cycoloy® C1000HF PC+ABS (Europe-Africa-Middle East)
CYCOLOY C1000HF is a general purpose PC+ABS blend specially developed for thin wall applications requiring a high flow with a good balance of properties. It is suitable for applications in the autom..
|
|||
| CTE, linear, Parallel to Flow |
80.0
µm/m-°C <br>@Temperature -40.0 - 40.0 °C
|
44.4
µin/in-°F <br>@Temperature -40.0 - 104 °F
|
ISO 11359-2 |
|
SABIC Innovative Plastics Cycoloy® FXC810MA PC+ABS (Europe-Africa-Middle East)
CYCOLOY FXC810MA is a multi-purpose PC+ABS injection moulding grade, suitable for those applications that require marble colour effects. The colour package may effect performance.This data was suppl..
|
|||
| CTE, linear, Parallel to Flow |
80.0
µm/m-°C <br>@Temperature 20.0 °C
|
44.4
µin/in-°F <br>@Temperature 68.0 °F
|
|
|
Ineos ABS Lustran® QE 1455, Injection Grade
(discontinued **)
Injection molding grade, increased heat resistance, medium gloss.Applications: Automotive: interior parts.Information provided by Bayer.LANXESS was spun-off from Bayer in early 2005. Business renam..
|
|||
| CTE, linear, Parallel to Flow |
80.0
µm/m-°C <br>@Temperature 20.0 °C
|
44.4
µin/in-°F <br>@Temperature 68.0 °F
|
|
|
Ineos ABS Lustran® QE 1455/L2, Injection Grade
(discontinued **)
Injection molding grade, increased heat resistance, medium gloss, UV-stabilized grade.Applications: Automotive: body parts.Information provided by Bayer.LANXESS was spun-off from Bayer in early 2005..
|
|||
| CTE, linear, Parallel to Flow |
80.0
µm/m-°C <br>@Temperature 23.0 - 55.0 °C
|
44.4
µin/in-°F <br>@Temperature 73.4 - 131 °F
|
ISO 11359-1, -2 |
|
Lanxess Durethan® B 31 FCS 000000 Nylon 6, Film Grade
PA 6, non-reinforced, extrusion, low viscosity, slip agentInformation provided by LANXESS.
|
|||
| CTE, linear, Parallel to Flow |
80.0
µm/m-°C <br>@Temperature 23.0 - 55.0 °C
|
44.4
µin/in-°F <br>@Temperature 73.4 - 131 °F
|
ISO 11359-1, -2 |
|
Lanxess Durethan® A 30 S FN31 000000 Nylon 66, Flame Retardant
PA 66, non-reinforced, injection molding, halogen-free flame retardant, improved flowabilityInformation provided by LANXESS.
|
|||
| CTE, linear, Parallel to Flow |
80.0
µm/m-°C <br>@Temperature -40.0 - 40.0 °C
|
44.4
µin/in-°F <br>@Temperature -40.0 - 104 °F
|
ISO 11359-2 |
|
SABIC Innovative Plastics NORYL PX9406P PPE+PS (Europe-Africa-Middle East) |
|||
| CTE, linear, Parallel to Flow |
80.0
-
110
µm/m-°C <br>@Temperature 23.0 - 80.0 °C
|
44.4
-
61.1
µin/in-°F <br>@Temperature 73.4 - 176 °F
|
ISO 11359-1/-2 |
|
Styrolution Luran® S KR 2859 UV ASA
Description: Stiff extrusions product, versatile grade for profile and sheet extrusion as protective cap layer.Information provided by STYROLUTION, which is a joint venture between BASF and INEOS
|
|||
| CTE, linear, Parallel to Flow |
80.0
-
110
µm/m-°C <br>@Temperature 23.0 - 80.0 °C
|
44.4
-
61.1
µin/in-°F <br>@Temperature 73.4 - 176 °F
|
ISO 11359-1/-2 |
|
Styrolution Terluran® SP-6 ABS
Description: High impact grade, suitable for extrusion.Information provided by STYROLUTION, which is a joint venture between BASF and INEOS
|
|||
| CTE, linear, Parallel to Flow |
80.0
µm/m-°C <br>@Temperature 20.0 °C
|
44.4
µin/in-°F <br>@Temperature 68.0 °F
|
ISO data |
|
Styron Magnumâ„¢ 941 ABS
MAGNUM® ABS resins are thermoplastic materials which provide an excellent balance of processability, impact resistance and heat resistance as imparted by the various polymer compositions. MAGNUM ..
|
|||
| CTE, linear, Parallel to Flow |
80.0
µm/m-°C <br>@Temperature 23.0 - 60.0 °C
|
44.4
µin/in-°F <br>@Temperature 73.4 - 140 °F
|
ISO 11359-2 |
|
SABIC Innovative Plastics Noryl GTX VP7133 PPE+PA (Europe-Africa-Middle East)
Noryl GTX VP7133 is an unfilled extrusion grade which offers high heat resistance in combination with high meltstrength.The material is especially designed for thermal break profiles which are used ..
|
|||
| CTE, linear, Parallel to Flow |
80.0
µm/m-°C <br>@Temperature 20.0 °C
|
44.4
µin/in-°F <br>@Temperature 68.0 °F
|
ISO data |
|
Styron Magnumâ„¢ 357HP ABS, High Heat
MAGNUM® ABS resins are thermoplastic materials which provide an excellent balance of processability, impact resistance and heat resistance as imparted by the various polymer compositions. MAGNUM ..
|
|||
| CTE, linear, Parallel to Flow |
80.0
µm/m-°C <br>@Temperature 20.0 °C
|
44.4
µin/in-°F <br>@Temperature 68.0 °F
|
ISO 11359-1/-2 |
|
DSM Stanyl® TW371 Nylon 46 (European and Asian Grade) (Dry)
Stanyl is a high performance polyamide providing good performance and value across a broad range of automotive and electronic applications. Stanyl offers:Highest mechanical properties at high temper..
|
|||
| CTE, linear, Parallel to Flow |
80.0
µm/m-°C <br>@Temperature 23.0 - 60.0 °C
|
44.4
µin/in-°F <br>@Temperature 73.4 - 140 °F
|
ISO 11359-2 |
|
Eurostar Staramide B28N PA6, Nucleated, Injection Molded
Staramide B28N is a Nucleated and Unreinforced Polyamide 6, Injection Molding ResinInformation provided by Eurostar.
|
|||
| CTE, linear, Parallel to Flow |
80.0
µm/m-°C <br>@Temperature 20.0 °C
|
44.4
µin/in-°F <br>@Temperature 68.0 °F
|
|
|
BASF Procom® D 1188 Polypropylene
Data was collected by ISO methods and provided by BASF.
|
|||
| CTE, linear, Parallel to Flow |
80.0
µm/m-°C <br>@Temperature 20.0 °C
|
44.4
µin/in-°F <br>@Temperature 68.0 °F
|
|
|
Arkema Group Cristamid® MS 1100 Semi-Aromatic Nylon (PASA) (Conditioned)
Designation ISO 1874-PA12/xx,MHLR,12-020Semi-aromatic polyamide (PASA) grade for injection molding and tubes extrusion.Transparency even thick. High resistance to environmental stress cracking. Good..
|
|||
| CTE, linear, Parallel to Flow |
80.0
µm/m-°C <br>@Temperature 20.0 °C
|
44.4
µin/in-°F <br>@Temperature 68.0 °F
|
|
|
BASF Procom® D 1133 Polypropylene
Data was collected by ISO methods and provided by BASF.
|
|||
| CTE, linear, Parallel to Flow |
80.0
µm/m-°C <br>@Temperature 20.0 °C
|
44.4
µin/in-°F <br>@Temperature 68.0 °F
|
|
|
BASF Procom® T20C 556 Polypropylene
Uses: car heater casings, electrical and domestic appliance components (e.g. motor housings, dryer drums), industrial and agricultural plant components, textile bobbins.Data was collected by ISO met..
|
|||
| CTE, linear, Parallel to Flow |
80.0
µm/m-°C <br>@Temperature 20.0 °C
|
44.4
µin/in-°F <br>@Temperature 68.0 °F
|
|
|
BASF Procom® T20C 557 Polypropylene
Car interior trim panels.Data was collected by ISO methods and provided by BASF.
|
|||
| CTE, linear, Parallel to Flow |
80.0
µm/m-°C <br>@Temperature 23.0 - 80.0 °C
|
44.4
µin/in-°F <br>@Temperature 73.4 - 176 °F
|
ISO 11359-2 |
|
SABIC Innovative Plastics NORYL PX2355 PPE+HIPS (Europe-Africa-Middle East)
NORYL PX2355 is an unfilled, medium heat, low odour and low emission material with excellent heat aging performance. It has been developed for automotive interior applications, such as instrument pa..
|
|||