Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Polymer Property : UL RTI, Mechanical without Impact = 149 °F Product List

Thermal Properties

Tips: 30 items are displayed at most.
Thermal Properties Metric English Comments
UL RTI, Mechanical without Impact 65.0 - 105 °C
149 - 221 °F
Average value: 77.7 °C Grade Count:14
Overview of materials for Polyphenylene Ether, Heat Resistant
This property data is a summary of similar materials in the MatWeb database for the category "Polyphenylene Ether, Heat Resistant". Each property range of values reported is minimum and maximum valu..
UL RTI, Mechanical without Impact 65.0 °C
<br>@Thickness 0.750 - 0.820 mm
149 °F
<br>@Thickness 0.0295 - 0.0323 in
LG Chemical LUMID GN1001BF PA66, Halogen Free Flame Retardant
Feature: Injection Molding, PA66, Halogen Free Flame RetardantApplication: ConnectorsCAS No. 32131-17-2, 25038-54-4 and 37640-57-6Information provided by LG Chemical
UL RTI, Mechanical without Impact 65.0 °C
<br>@Thickness >=0.750 mm
149 °F
<br>@Thickness >=0.0295 in
LG Chemical LUMID GP2130A(W) PA6+GF13%, General Purpose
Feature: Injection Molding, PA6+GF13%, General PurposeApplication: Automotive PartsCAS No. 25038-54-4 and 65997-17-3Information provided by LG Chemical
UL RTI, Mechanical without Impact 65.0 °C
<br>@Thickness >=0.750 mm
149 °F
<br>@Thickness >=0.0295 in
LG Chemical LUMID GP2200A(W) PA6+GF20%, General Purpose
Feature: Injection Molding, PA6+MF23%, High ImpactPA6+GF20%, General PurposeApplication: HMID, SLMP B, HolderCAS No. 32131-17-2 and 65997-17-3Information provided by LG Chemical
UL RTI, Mechanical without Impact 65.0 °C
<br>@Thickness >=0.750 mm
149 °F
<br>@Thickness >=0.0295 in
LG Chemical LUMID GP2500A(W) PA6+GF50%, General Purpose
Feature: Injection Molding, PA6+GF50%, General PurposeApplication: Automotive (Gear Shift Housing)CAS No. 25038-54-4 and 65997-17-3Information provided by LG Chemical
UL RTI, Mechanical without Impact 65.0 °C
<br>@Thickness >=0.750 mm
149 °F
<br>@Thickness >=0.0295 in
LG Chemical LUMID GP3200A(W) PA6+MF20%, General Purpose
Feature: Injection Molding, PA6+MF23%, High ImpactPA6+MF15%, General PurposeApplication: E&E (Rice Cooer Housing)CAS No. 25038-54-4 and 9010-79-1Information provided by LG Chemical
UL RTI, Mechanical without Impact 65.0 °C
<br>@Thickness >=1.50 mm
149 °F
<br>@Thickness >=0.0591 in
LG Chemical LUPOL GP3200 PP+MF20%
Description: Injection Molding, PP+MF10%, General PurposeApplication: Electrical & Electronic, Automotive PartsCAS: 9003-07-0 and 14807-96-6Information provided by LG Chemical
UL RTI, Mechanical without Impact 65.0 °C
<br>@Thickness >=1.50 mm
149 °F
<br>@Thickness >=0.0591 in
LG Chemical LUPOL GP3202 PP+MF20%
Description: Injection Molding, PP+MF10%, General Purpose, Good WeatherabilityApplication: Electrical, Electronic and Automotive Interior PartsCAS: 9003-07-0 and 14807-96-6Information provided by LG..
UL RTI, Mechanical without Impact 65.0 °C
<br>@Thickness >=1.50 mm
149 °F
<br>@Thickness >=0.0591 in
LG Chemical LUPOL GP3302 PP+MF30%
Description: Injection Molding, PP+MF30%, General Purpose, Good WeatherabilityApplication: Electrical, Electronic and Automotive Interior PartsCAS: 9003-07-0 and 14807-96-6Information provided by LG..
UL RTI, Mechanical without Impact 65.0 °C
149 °F
UL 746B
SABIC Innovative Plastics LNP Thermocomp RF006XXP PA 66 (Europe-Africa-Middle East)
30% glass fibre reinforced Polyamide 66 injection moulding resin.This data was supplied by SABIC-IP for the Europe-Africa-Middle East region.
UL RTI, Mechanical without Impact 65.0 °C
149 °F
UL 746B
SABIC Innovative Plastics NORYL NH6010B PPE+HIPS (Asia Pacific)
Noryl* NH6010B resin is a high performance, modified PPE-PS blend that exhibits an excellent balance of lower smoke production upon burning, nonhalogenated flame retardance and low specific gravity...
UL RTI, Mechanical without Impact 65.0 °C
149 °F
UL 746B
SABIC Innovative Plastics NORYL NH6010B PPE+HIPS (Europe-Africa-Middle East)
Noryl* NH6010B resin is a high performance, modified PPE-PS blend that exhibits an excellent balance of lower smoke production upon burning, nonhalogenated flame retardance and low specific gravity...
UL RTI, Mechanical without Impact 65.0 °C
149 °F
UL 746B
SABIC Innovative Plastics LNP Thermocomp R1000HI620 PA 66 (Europe-Africa-Middle East)
Impact modified Polyamide 66 injection moulding resin.This data was supplied by SABIC-IP for the Europe-Africa-Middle East region.
UL RTI, Mechanical without Impact 65.0 °C
<br>@Thickness 0.749 mm
149 °F
<br>@Thickness 0.0295 in
UL 746
Teknor Apex Chemlon® 125-15 MGH Nylon 66, 25% Mineral Reinforced, 15% Glass Fiber Reinforced
Notes: 25% Mineral - 15% Glass; Excellent stiffness and strength, especially at high temperatures, with improved warpage control over glass reinforced products; FMVSS Flammability: Passes, FMVSS 302..
UL RTI, Mechanical without Impact 65.0 °C
149 °F
UL 746B
SABIC Innovative Plastics NORYL ENV150 PPE (Europe-Africa-Middle East)
Noryl* ENV150 modified polyphenylene ether resin is an unfilled, flame retardant high heat grade suitable for extrusion molding conversion route. It uses non-chlorinated, non-brominated FR additives..
UL RTI, Mechanical without Impact 65.0 °C
149 °F
UL 746B
SABIC Innovative Plastics Noryl FXN2090H PPE+HIPS (Europe-Africa-Middle East)
Noryl* FXN2090H resin is an unfilled, injection moldable grade. Designed for exceptionally high gloss and improved pencil hardness vs. standard Noryl grades, FXN2090H resin uses non-halogenated FR a..
UL RTI, Mechanical without Impact 65.0 °C
149 °F
UL 746B
SABIC Innovative Plastics NORYL GFN1720 PPE+HIPS (Asia Pacific)
Noryl* GFN1720 is a 20% glass fiber reinforced, injection moldable grade. This modified polyphenylene ether resin is designed to deliver a balance of heat, strength and electrical properties. Noryl ..
UL RTI, Mechanical without Impact 65.0 °C
<br>@Thickness 0.780 mm
149 °F
<br>@Thickness 0.0307 in
UL 746
A. Schulman POLYFLAM™ FPP 1006S Talc Filled Homopolymer Polypropylene
DescriptionPolyfort® FPP 1006S is a 20% talc filled homopolymer polypropylene compound formulated with an internal mold release. Information provided by A. Schulman.
UL RTI, Mechanical without Impact 65.0 °C
149 °F
Eurostar Staramide A28N PA66, Nucleated, Injection Molding
Staramide A28K is an Unreinforced and Heat Stabilized, Polyamide 66, Injection Molding ResinInformation provided by Eurostar.
UL RTI, Mechanical without Impact 65.0 °C
149 °F
Eurostar Staramide B28H PA6, Heat Stabilized, Injection Molded
Staramide B28H is a Heat Stabilized, Unreinforced Polyamide 6, Injection Molding ResinInformation provided by Eurostar.
UL RTI, Mechanical without Impact 65.0 °C
149 °F
Eurostar Staramide RF006SXP PA66, 30% Glass Fiber Filled, Injection Molded
Staramide RF006SXP is a 30% Glass Fiber Reinforced Polyamide 66 Injection Molding Resin (also known as RF1006HS)Information provided by Eurostar.
UL RTI, Mechanical without Impact 65.0 °C
149 °F
Eurostar Staramide RF006SXS PA66, 30% Glass Fiber Filled, Injection Molded
Staramide RF006SXS is a 30% Glass Fiber Reinforced Polyamide 66 Injection Molding Resin (also known as RF1006HS)Information provided by Eurostar.
UL RTI, Mechanical without Impact 65.0 °C
149 °F
Eurostar Starflam BFR460B1 PA6, Glass Fiber Filled, Flame Retardant, Injection Molded
Starflam BFR460B1 is a Flame Retardant, Glass Fiber Reinforced Polyamide 6, Injection Molding ResinInformation provided by Eurostar.
UL RTI, Mechanical without Impact 65.0 °C
149 °F
Eurostar Starflam BFR552Y6 PA6, Mineral/Glass Fiber Filled, Flame Retardant, Injection Molded
Starflam BFR552Y6 is a Halogen and Red Phosphorous Free, Flame Retardant, Glass Fiber Reinforced, Mineral Filled, Polyamide 6, Injection Molding ResinInformation provided by Eurostar.
UL RTI, Mechanical without Impact 65.0 °C
<br>@Thickness 1.60 mm
149 °F
<br>@Thickness 0.0630 in
Eurostar Starflam PK0022E PA6, 10% Mineral Filled, Injection Molded
PK0022E is a Halogen Free and Phosphorous Free, Mineral Filed, Polyamide 6 Injection Molding (also known as PM3620Z22 or PA 10E6 U9 Z22)Information provided by Polymer Technology & Services, the Nor..
UL RTI, Mechanical without Impact 65.0 °C
149 °F
Eurostar Starflam RF0069 PA66, 30% Glass Fiber, Flame Retardant, Injection Molded
Starflam RF0069 is a Flame Retardant, 30% Glass Reinforced Polyamide 66 Injection Molding Resin (also known as PA66 30V U2 Z79 or RF1006Z590)Information provided by Eurostar.
UL RTI, Mechanical without Impact 65.0 °C
149 °F
Eurostar Starflam AFR460B PA66, Glass Fiber Reinforced, Flame Retardant, Injection Molding
Starflam AFR460B is a Flame Retardant, Glass Fiber Reinforced Polyamide 66, Injection Molding ResinInformation provided by Eurostar.
UL RTI, Mechanical without Impact 65.0 °C
149 °F
Arkema Group Rilsan® BZM 8 NOIR TL Nylon 11, 8% Glass Fiber Filled (Conditioned)
Designation ISO 1874-PA11,MHL,18-020,GF8Rigid grade with glass fiber (8%) filler for injection molding. Available color: black. Light and heat stabilized.Rigidity. Outstanding compromise between goo..
UL RTI, Mechanical without Impact 65.0 °C
<br>@Thickness 1.50 mm
149 °F
<br>@Thickness 0.0591 in
746B
BASF Ultramid® TG3S 15% Glass Filled PA6 (Dry)
Description: Ultramid TG3S is a 15% glass reinforced, heat stabilized, impact modified PA6 injection molding compound developed for applications requiring improved toughness in combination with a ba..
UL RTI, Mechanical without Impact 65.0 °C
149 °F
UL 746B
SABIC Innovative Plastics NORYL RN0611 PPE+HIPS (Europe-Africa-Middle East)
Noryl RN0611 is an unfilled Post Consumer recycle (PCR) based injection moldable modified polyphenylene ether resin comprising at least 30% PCR styrenic series resin content. Designed for good dimen..
Copyright © lookpolymers.com All Rights Reserved