Physical Properties Metric English Comments
Density 4.45 g/cc
0.161 lb/in³
Mechanical Properties Metric English Comments
Knoop Microhardness 666
666
.1/20
Modulus of Elasticity 124 GPa
18000 ksi
Poissons Ratio 0.298
0.298
Shear Modulus 48.0 GPa
6960 ksi
calculated
Thermal Properties Metric English Comments
CTE, linear 6.00 µm/m-°C

@Temperature -30.0 - 70.0 °C
3.33 µin/in-°F

@Temperature -22.0 - 158 °F
7.20 µm/m-°C

@Temperature 20.0 - 300 °C
4.00 µin/in-°F

@Temperature 68.0 - 572 °F
Specific Heat Capacity 0.540 J/g-°C
0.129 BTU/lb-°F
Thermal Conductivity 0.910 W/m-K
6.32 BTU-in/hr-ft²-°F
Transformation Temperature, Tg 638 °C
1180 °F
Optical Properties Metric English Comments
Refractive Index 1.90366

@Wavelength 587.6 nm
1.90366

@Wavelength 587.6 nm
n<sub>d</sub>
1.91048

@Wavelength 546.1 nm
1.91048

@Wavelength 546.1 nm
n<sub>e</sub>
Transmission, Visible 50.4 %

@Thickness 10.0 mm,
Wavelength 380 nm
50.4 %

@Thickness 0.394 in,
Wavelength 380 nm
84.7 %

@Thickness 10.0 mm,
Wavelength 405 nm
84.7 %

@Thickness 0.394 in,
Wavelength 405 nm
95.9 %

@Thickness 10.0 mm,
Wavelength 460 nm
95.9 %

@Thickness 0.394 in,
Wavelength 460 nm
99.3 %

@Thickness 10.0 mm,
Wavelength 580 nm
99.3 %

@Thickness 0.394 in,
Wavelength 580 nm
99.6 %

@Thickness 10.0 mm,
Wavelength 700 nm
99.6 %

@Thickness 0.394 in,
Wavelength 700 nm
IR Transmittance 55.6 %

@Thickness 10.0 mm,
Wavelength 2500 nm
55.6 %

@Thickness 0.394 in,
Wavelength 2500 nm
99.1 %

@Thickness 10.0 mm,
Wavelength 1530 nm
99.1 %

@Thickness 0.394 in,
Wavelength 1530 nm
UV Transmittance 5.0 %

@Thickness 10.0 mm,
Wavelength 365 nm
5.0 %

@Thickness 0.394 in,
Wavelength 365 nm
18.1 %

@Thickness 10.0 mm,
Wavelength 370 nm
18.1 %

@Thickness 0.394 in,
Wavelength 370 nm
Chemical Properties Metric English Comments
Acid Class, SR 3.0
3.0
Alkali Class, AR 1.0
1.0
Stain Resistance Class, FR 0.00
0.00
Descriptive Properties Value Comments
B 0
Climatic Resistance Test CR 1
HG 1
K (10-6mm2/N) 1.64
Phosphate Resistance PR 1
T1013.0 (°C) 639
T107.6 (°C) 733