Material Notes:
Product Description: Bicor AB-X is a two-side coated, sealable OPP film designed for general use in many applications, including overwrap, horizontal and vertical packaging. This film is suitable as an unsupported web or in a lamination. It can be surface printed, reverse printed, or used unprinted.Availability: Latin America, North America and South AmericaKey Features:Outstanding optical propertiesRobust machinablityLow and consistent COFExcellent hot slipExcellent flavor and aroma barrierExcellent hot tack and seal strengthPrintable on both sidesFeatures:Acrylic CoatedFlavor & Aroma BarrierIn Lamination Lap SealableApplications:Biscuits/Cookie/CrackersBox OverwrapConfectionery, GumConfectionery, SugarTobaccoUses:Box Overwrap Flexible PackagingHFF Flexible PackagingPre-made Bags - Flexible PackagingTobacco Overwrap Flexible PackagingVFFS Flexible PackagingProcessing Method: Cold Seal Adhesive, Inner Web Adhesive Lamination, Outer Web Adhesive Lamination, Solvent Flexographic Printing, Solvent Rotogravure Printing, Surface Print Unsupported and Water-based Flexographic Printing Information provided by ExxonMobil Chemical
Physical Properties Metric English Comments
Water Vapor Transmission 5.70 g/m²/day
0.367 g/100 in²/day
38°C, 90% RH; ExxonMobil Method
Thickness 25.4 microns
1.00 mil
Nominal; ExxonMobil Method
Coating Weight 22.2 g/m²
13.9 lb/ream
ExxonMobil Method
Mechanical Properties Metric English Comments
Coefficient of Friction 0.24
0.24
ExxonMobil Method
Film Tensile Strength at Break, MD 137 MPa
19900 psi
ExxonMobil Method
Film Tensile Strength at Break, TD 222 MPa
32200 psi
ExxonMobil Method
Thermal Properties Metric English Comments
Shrinkage, MD 4.5 %
4.5 %
at 275°F; ExxonMobil Method
Shrinkage, TD 4.0 %
4.0 %
at 275°F; ExxonMobil Method
Optical Properties Metric English Comments
Haze 1.7 %
1.7 %
ExxonMobil Method
Gloss 87 %
87 %
ExxonMobil Method
Descriptive Properties Value Comments
Crimp Seal MST 205°F
Crimp Seal Strength 560, g/in
260°F, 20psi, 3/4sec
Yield 31000 in2/lb