Material Notes:
Information provided by Multibase
Mechanical Properties Metric English Comments
Hardness, Shore A 67
67
as molded
72
72
post cured- 2 hours at 177°C
75
75
post cured- 4 hours at 204°C
Tensile Strength, Ultimate 7.136 MPa
1035 psi
post cured- 4 hours at 204°C
7.667 MPa
1112 psi
as molded
7.79 MPa
1130 psi
post cured- 2 hours at 177°C
Tensile Strength, Yield 3.45 MPa
500 psi
at 200%, as molded
3.52 MPa
510 psi
at 200%, post cured- 2 hours at 177°C
3.73 MPa
541 psi
200%, post cured- 4 hours at 204°C
Elongation at Break 552 %
552 %
post cured- 4 hours at 204°C
672 %
672 %
post cured- 2 hours at 177°C
772 %
772 %
as molded
Tear Strength 40.8 kN/m
233 pli
post cured- 4 hours at 204°C; Die B
41.7 kN/m
238 pli
post cured- 2 hours at 177°C; Die B
43.1 kN/m
246 pli
as molded; Die B