Material Notes:
Applications & Industries: General: Carbon / Coke (soft) filler is good in dry running conditions, adds to the creep resistance, increases the hardness and raises the thermal conductivity of PTFE; Carbon / Coke (soft) compounds have good wear properties, but has low tool wear during machining, thus allowing machining to very close tolerances; Carbon / Coke (soft) compounds have some electrical conductivity and are therefore antistatic; and Carbon filled compounds when combined with graphite, have excellent wear properties. The combination of the above properties makes carbon / graphite compounds the preferred material for non - lubricated piston rings. Chemical: Dynamic & shaft seals and Seals & gaskets. Flat gaskets are used to seal flanges in pipelines.Construction: Bridge bearings. Slide bearings.Engineering: Anti - friction bearing cages & bearing plates; Bearings, bushes, shaft bearings / seals (in combustion engines); Film bearings. Multi - layer composite bearings. Fabric bearings; Laboratory equipment. Measuring & control technology; Pipe supports. Expansion bellows. Glandless valves & pumps, valve seats; Piston rings in hydraulic systems and compressors; and Piston rod packings used in compressor plunger pumps & valves.CHEMICAL RESISTANCE: The strength of the carbon - fluorine bond and the shielding of the carbon chains by the fluorine atoms result in a chemical inertness which is virtually universal, except alkali metals, fluorine under certain conditions, some fluorine compounds & halogen gases at elevated temperatures. Carbon / Coke is a good inert filler, except in oxidising environments where glass performs better. Resistant to hydrofluoric acid.Information provided by Dalau
Physical Properties Metric English Comments
Density 2.05 - 2.13 g/cc
0.0741 - 0.0770 lb/in³
BS2782:Pt6
Deformation 4.8 %

@Time 3600 sec,
Pressure 14.2 MPa
4.8 %

@Time 1.00 hour,
Pressure 2060 psi
ASTM D621
6.6 %

@Pressure 14.2 MPa,
Time 86400 sec
6.6 %

@Pressure 2060 psi,
Time 24.0 hour
ASTM D621
6.6 %

@Time 3600 sec,
Pressure 5.00 MPa
6.6 %

@Time 1.00 hour,
Pressure 725 psi
150°C; ASTM D621
Mechanical Properties Metric English Comments
Hardness, Shore D 70 - 72
70 - 72
ASTM D2240
Tensile Strength 12.0 - 25.0 MPa
1740 - 3630 psi
Moulding Direction; BS2782:Pt3
Elongation at Break 50 - 250 %
50 - 250 %
Moulding Direction; BS2782:Pt3
Flexural Yield Strength 10.3 MPa

@Strain 0.200 %
1490 psi

@Strain 0.200 %
ASTM D790
Flexural Modulus 1.09 GPa
158 ksi
ASTM D790
Compressive Strength 2.30 MPa

@Strain 0.200 %,
Temperature 150 °C
334 psi

@Strain 0.200 %,
Temperature 302 °F
ASTM D695
9.13 MPa

@Strain 0.200 %,
Temperature 23.0 °C
1320 psi

@Strain 0.200 %,
Temperature 73.4 °F
ASTM D695
Thermal Properties Metric English Comments
Thermal Conductivity 0.580 W/m-K
4.03 BTU-in/hr-ft²-°F
Moulding Direction; ASTM C177
Melting Point 327 °C
621 °F
ASTM D3417
Maximum Service Temperature, Air 260 °C
500 °F
300 °C
572 °F
Short Periods
Minimum Service Temperature, Air -200 °C
-328 °F
Flash Point 630 °C
1170 °F
ASTM D1929
Oxygen Index 98 - 100 %
98 - 100 %
ASTM D2863
Descriptive Properties Value Comments
Color Black
Users viewing this material also viewed the following: