PTS PPE-LXS 314-30 PPE-HIPS, 30% Glass Filled

Category Polymer , Thermoplastic , Polyphenylene Ether/PPO , Polystyrene (PS) , Polystyrene + Polyphenylene Ether, Glass Filler
Manufacturer Polymer Technology & Services, LLC (PTS)
Trade Name
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF PTS PPE-LXS 314-30 PPE-HIPS, 30% Glass Filled.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
Typical Applications: Water industrial partsInformation provided by PTS LLC.
Physical Properties Metric English Comments
Specific Gravity 1.35 g/cc
1.35 g/cc
ASTM D792
Water Absorption 0.10 %

@Temperature 23.0 °C,
Time 86400 sec
0.10 %

@Temperature 73.4 °F,
Time 24.0 hour
ASTM D570
Linear Mold Shrinkage, Flow 0.0030 - 0.0050 cm/cm
0.0030 - 0.0050 in/in
ASTM D955
Melt Flow 15 g/10 min

@Load 5.00 kg,
Temperature 300 °C
15 g/10 min

@Load 11.0 lb,
Temperature 572 °F
ASTM D1238
Mechanical Properties Metric English Comments
Tensile Strength at Break 110 MPa
16000 psi
type I; ASTM D638
Elongation at Break 6.0 %
6.0 %
type I; ASTM D638
Flexural Strength 160 MPa
23200 psi
2.6 mm/min; ASTM D790
Flexural Modulus 5.50 GPa
798 ksi
2.6 mm/min; ASTM D790
Izod Impact, Notched (ISO) 14.0 kJ/m²
6.66 ft-lb/in²
ASTM D256
Thermal Properties Metric English Comments
Deflection Temperature at 1.8 MPa (264 psi) 135 °C

@Thickness 6.40 mm
275 °F

@Thickness 0.252 in
ASTM D648