Hogen Durakut H15W 68 Tungsten/32 Copper PM Metal Composite

Category Metal , Metal Matrix Composite , Nonferrous Metal , Refractory Metal , Tungsten Alloy
Manufacturer Hogen Industries
Trade Name Durakut
Port Shanghai port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Hogen Durakut H15W 68 Tungsten/32 Copper PM Metal Composite.pdf
Price EMAIL US    sales@lookpolymers.com
Material Notes:
RWMA Class ECM-EDMDURAKUT Copper-Tungsten and Silver-Tungsten are manufactured as electrode materials for EDM (Electrical Discharge Machining), ECM (Electro Chemical Machining) and ECD (Electro Chemical Deburring).Hogan DURAKUT materials are also manufactured by the powder metallurgy techniques of pressing, sintering and infiltrating tungsten with copper or silver. DURAKUT is produced under the same rigid manufacturing procedures and strict quality control supervision as Duralloy. This assures a high performance electrode providing greater cutting stability, excellent machinability and reduced down time. For extremely close tolerance work, Durakut holds dimensions and will not break down due to porosity and other structural deficiencies sometimes found in other Copper-Tungsten electrode alloys.DURAKUT Copper-Tungsten is well suited for machining carbide dies. Further more, it offers greater cutting stability in machining refractory metals and exotics.Tungsten alloys used for EDM and ECM applications are far superior when fine surface finishes, deep narrow slots or ribs and small precise holes are required. Tungsten alloys are preferred when matching extremely detailed sections. In the ECM process, Copper-Tungsten withstands erosive effects of short circuit malfunctions far better than other materials.Data provided by Hogen Industries.
Physical Properties Metric English Comments
Density >= 13.8 g/cc
>= 0.499 lb/in³
Mechanical Properties Metric English Comments
Hardness, Rockwell B 83
83
Tensile Strength, Ultimate 517 MPa
75000 psi
Thermal Properties Metric English Comments
CTE, linear 10.77 µm/m-°C

@Temperature 20.0 °C
5.983 µin/in-°F

@Temperature 68.0 °F
Specific Heat Capacity 0.214 J/g-°C

@Temperature 20.0 °C
0.0511 BTU/lb-°F

@Temperature 68.0 °F
Thermal Conductivity 201 W/m-K

@Temperature 20.0 - 400 °C
1390 BTU-in/hr-ft²-°F

@Temperature 68.0 - 752 °F
Component Elements Properties Metric English Comments
Copper, Cu 32 %
32 %
Tungsten, W 68 %
68 %
Electrical Properties Metric English Comments
Electrical Resistivity 0.00000360 ohm-cm
0.00000360 ohm-cm