| Category | Metal , Ferrous Metal , Austenitic , Stainless Steel |
| Manufacturer | Outokumpu |
| Trade Name | |
| Port | Ningbo port,China |
| Trade Terms | FOB, CFR, CIF |
| Payment Terms | L/C, T/T, Western Union |
| Download PDF | Outokumpu 4301 Cr-Ni Austenitic Stainless Steel.pdf |
| Price | EMAIL US sales@lookpolymers.com |
| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Density | 7.90 g/cc | 0.285 lb/in³ | RT |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Hardness, Brinell | 165 | 165 | Outokumpu Typical, 20°C, Hot rolled plate (Quarto); EN 10003-1 |
| 175 | 175 | Outokumpu Typical, 20°C, Cold rolled strip/sheet; EN 10003-1 | |
| Tensile Strength, Ultimate | >= 520 MPa | >= 75400 psi | EN 10002-1 |
| 600 MPa | 87000 psi | Outokumpu Typical, Hot Rolled Plate (Quarto); EN 10002-1 | |
| 360 MPa @Temperature 500 °C |
52200 psi @Temperature 932 °F |
EN min.; EN 10002-5 | |
| 380 MPa @Temperature 300 °C |
55100 psi @Temperature 572 °F |
EN min.; EN 10002-5 | |
| 380 MPa @Temperature 400 °C |
55100 psi @Temperature 752 °F |
EN min.; EN 10002-5 | |
| 400 MPa @Temperature 200 °C |
58000 psi @Temperature 392 °F |
EN min.; EN 10002-5 | |
| 450 MPa @Temperature 100 °C |
65300 psi @Temperature 212 °F |
EN min.; EN 10002-5 | |
| 860 MPa @Temperature -80.0 °C |
125000 psi @Temperature -112 °F |
EN min; EN 10002-5 | |
| 1250 MPa @Temperature -196 °C |
181000 psi @Temperature -321 °F |
EN min; EN 10002-5 | |
| Tensile Strength, Yield | 210 MPa @Strain 0.200 % |
30500 psi @Strain 0.200 % |
EN min.,RT; EN 10002-1 |
| 250 MPa @Strain 1.00 % |
36300 psi @Strain 1.00 % |
EN min.,RT; EN 10002-1 | |
| 290 MPa @Strain 0.200 % |
42100 psi @Strain 0.200 % |
Outokumpu Typical,Cold Rolled Strip/Sheet; EN 10002-1 | |
| 330 MPa @Strain 1.00 % |
47900 psi @Strain 1.00 % |
Outokumpu Typical,Cold Rolled Strip/Sheet; EN 10002-1 | |
| 92.0 MPa @Strain 0.200 %, Temperature 500 °C |
13300 psi @Strain 0.200 %, Temperature 932 °F |
EN min.; EN 10002-5 | |
| 98.0 MPa @Strain 0.200 %, Temperature 400 °C |
14200 psi @Strain 0.200 %, Temperature 752 °F |
EN min.; EN 10002-5 | |
| 110 MPa @Strain 0.200 %, Temperature 300 °C |
16000 psi @Strain 0.200 %, Temperature 572 °F |
EN min.; EN 10002-5 | |
| 120 MPa @Strain 1.00 %, Temperature 500 °C |
17400 psi @Strain 1.00 %, Temperature 932 °F |
EN min.; EN 10002-5 | |
| 125 MPa @Strain 1.00 %, Temperature 400 °C |
18100 psi @Strain 1.00 %, Temperature 752 °F |
EN min.; EN 10002-5 | |
| 127 MPa @Strain 0.200 %, Temperature 200 °C |
18400 psi @Strain 0.200 %, Temperature 392 °F |
EN min.; EN 10002-5 | |
| 135 MPa @Strain 1.00 %, Temperature 300 °C |
19600 psi @Strain 1.00 %, Temperature 572 °F |
EN min.; EN 10002-5 | |
| 157 MPa @Strain 1.00 %, Temperature 200 °C |
22800 psi @Strain 1.00 %, Temperature 392 °F |
EN min.; EN 10002-5 | |
| 157 MPa @Strain 0.200 %, Temperature 100 °C |
22800 psi @Strain 0.200 %, Temperature 212 °F |
EN min.; EN 10002-5 | |
| 191 MPa @Strain 1.00 %, Temperature 100 °C |
27700 psi @Strain 1.00 %, Temperature 212 °F |
EN min.; EN 10002-5 | |
| 270 MPa @Strain 0.200 %, Temperature -80.0 °C |
39200 psi @Strain 0.200 %, Temperature -112 °F |
EN min.; EN 10002-5 | |
| 300 MPa @Strain 0.200 %, Temperature -196 °C |
43500 psi @Strain 0.200 %, Temperature -321 °F |
EN min.; EN 10002-5 | |
| 350 MPa @Strain 1.00 %, Temperature -80.0 °C |
50800 psi @Strain 1.00 %, Temperature -112 °F |
EN min.; EN 10002-5 | |
| 400 MPa @Strain 1.00 %, Temperature -196 °C |
58000 psi @Strain 1.00 %, Temperature -321 °F |
EN min.; EN 10002-5 | |
| Elongation at Break | >= 45.0 % | >= 45.0 % | EN 10002-1 |
| 55 % | 55 % | Outokumpu Typical, Hot Rolled Plate (Quarto); EN 10002-1 | |
| 30 % @Temperature -196 °C |
30 % @Temperature -321 °F |
EN min | |
| 35 % @Temperature -80.0 °C |
35 % @Temperature -112 °F |
EN min | |
| Modulus of Elasticity | 200 GPa | 29000 ksi | RT |
| 165 GPa @Temperature 500 °C |
23900 ksi @Temperature 932 °F |
||
| 172 GPa @Temperature 400 °C |
24900 ksi @Temperature 752 °F |
||
| 179 GPa @Temperature 300 °C |
26000 ksi @Temperature 572 °F |
||
| 186 GPa @Temperature 200 °C |
27000 ksi @Temperature 392 °F |
||
| 194 GPa @Temperature 100 °C |
28100 ksi @Temperature 212 °F |
||
| Poissons Ratio | 0.30 | 0.30 | RT |
| Shear Modulus | 77.0 GPa | 11200 ksi | calculated |
| Impact Test | >= 60.0 J | >= 44.3 ft-lb | Hot rolled plate/Cold rolled strip/sheet, 10x10mm test pieces; EN 10045-1 |
| Thermal Properties | Metric | English | Comments |
|---|---|---|---|
| CTE, linear | 16.0 µm/m-°C @Temperature 100 °C |
8.89 µin/in-°F @Temperature 212 °F |
|
| 16.5 µm/m-°C @Temperature 200 °C |
9.17 µin/in-°F @Temperature 392 °F |
||
| 17.0 µm/m-°C @Temperature 300 °C |
9.44 µin/in-°F @Temperature 572 °F |
||
| 17.5 µm/m-°C @Temperature 400 °C |
9.72 µin/in-°F @Temperature 752 °F |
||
| 18.0 µm/m-°C @Temperature 500 °C |
10.0 µin/in-°F @Temperature 932 °F |
||
| Specific Heat Capacity | 0.500 J/g-°C | 0.120 BTU/lb-°F | RT |
| Thermal Conductivity | 15.0 W/m-K | 104 BTU-in/hr-ft²-°F | RT |
| 20.0 W/m-K @Temperature 400 °C |
139 BTU-in/hr-ft²-°F @Temperature 752 °F |
| Component Elements Properties | Metric | English | Comments |
|---|---|---|---|
| Carbon, C | 0.040 % | 0.040 % | |
| Chromium, Cr | 18.1 % | 18.1 % | |
| Iron, Fe | 73.56 % | 73.56 % | |
| Nickel, Ni | 8.3 % | 8.3 % |
| Electrical Properties | Metric | English | Comments |
|---|---|---|---|
| Electrical Resistivity | 0.0000730 ohm-cm | 0.0000730 ohm-cm | RT |