| Category | Polymer , Thermoplastic , Polyphenylene Sulfide (PPS) , Polyphenylene Sulfide (PPS), Unreinforced, Extruded |
| Manufacturer | Quadrant Engineering Plastics Products |
| Trade Name | Techtron® |
| Port | Shanghai port,China |
| Trade Terms | EXW, FOB, CFR, CIF |
| Payment Terms | L/C, T/T, PayPal |
| Download PDF | Quadrant EPP Techtron® 1000 PPS Extruded Polyphenylene Sulfide (ASTM Product Data Sheet).pdf |
| Price | EMAIL US sales@lookpolymers.com |
| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Specific Gravity | 1.35 g/cc | 1.35 g/cc | ASTM D792 |
| Water Absorption | 0.010 % | 0.010 % | Immersion, 24hr; ASTM D570(2) |
| Water Absorption at Saturation | 0.030 % | 0.030 % | Immersion; ASTM D570(2) |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Hardness, Rockwell M | 95 | 95 | ASTM D785 |
| Hardness, Rockwell R | 125 | 125 | ASTM D785 |
| Hardness, Shore D | 85 | 85 | ASTM D2240 |
| Tensile Strength | 93.1 MPa | 13500 psi | ASTM D638 |
| Elongation at Break | 15 % | 15 % | ASTM D638 |
| Tensile Modulus | 3.45 GPa | 500 ksi | ASTM D638 |
| Flexural Strength | 145 MPa | 21000 psi | ASTM D790 |
| Flexural Modulus | 3.96 GPa | 575 ksi | ASTM D790 |
| Compressive Strength | 148 MPa | 21500 psi | 10% Def.; ASTM D695 |
| Compressive Modulus | 2.96 GPa | 430 ksi | ASTM D695 |
| Shear Strength | 62.1 MPa | 9000 psi | ASTM D732 |
| Izod Impact, Notched | 0.320 J/cm | 0.600 ft-lb/in | ASTM D256 Type A |
| Coefficient of Friction, Dynamic | 0.40 | 0.40 | Dry vs. Steel; QTM55007 |
| K (wear) Factor | 4830 x 10<sup>-8</sup> mm³/N-M | 2400 x 10<sup>-10</sup> in³-min/ft-lb-hr | QTM 55010 |
| Limiting Pressure Velocity | 0.105 MPa-m/sec | 3000 psi-ft/min | 4:1 safety factor; QTM 55007 |
| Thermal Properties | Metric | English | Comments |
|---|---|---|---|
| CTE, linear | 50.4 µm/m-°C @Temperature -40.0 - 149 °C |
28.0 µin/in-°F @Temperature -40.0 - 300 °F |
ASTM E831 |
| Thermal Conductivity | 0.288 W/m-K | 2.00 BTU-in/hr-ft²-°F | ASTM F433 |
| Melting Point | 282 °C | 540 °F | Crystalline, Peak; ASTM D3418 |
| Maximum Service Temperature, Air | 218 °C | 425 °F | Long Term |
| Deflection Temperature at 1.8 MPa (264 psi) | 121 °C | 250 °F | ASTM D648 |
| Flammability, UL94 | V-0 | V-0 | 1/8 inch (Estimated Rating) |
| Electrical Properties | Metric | English | Comments |
|---|---|---|---|
| Surface Resistivity per Square | >= 1.00e+13 ohm | >= 1.00e+13 ohm | EOS/ESD S11.11 |
| Dielectric Constant | 3.0 @Frequency 1e+6 Hz |
3.0 @Frequency 1e+6 Hz |
ASTM D150 |
| Dielectric Strength | 21.3 kV/mm | 540 kV/in | Short Term; ASTM D149 |
| Dissipation Factor | 0.0013 @Frequency 1e+6 Hz |
0.0013 @Frequency 1e+6 Hz |
ASTM D150 |
| Compliance Properties | Metric | English | Comments |
|---|---|---|---|
| 3A-Dairy | Yes | Yes | |
| Canada AG | No | No | |
| FDA | Yes | Yes | |
| NSF | No | No | |
| USDA | No | No | |
| USP Class VI | No | No |
| Chemical Resistance Properties | Metric | English | Comments |
|---|---|---|---|
| Acids, Strong (pH 1-3) | Limited | Limited | |
| Acids, Weak | Acceptable | Acceptable | |
| Alcohols | Acceptable | Acceptable | |
| Alkalies, Strong (pH 11-14) | Acceptable | Acceptable | |
| Alkalies, Weak | Acceptable | Acceptable | |
| Chlorinated Solvents | Acceptable | Acceptable | |
| Conductive / Static Dissipative | No | No | |
| Continuous Sunlight | Limited | Limited | |
| Hot Water / Steam | Acceptable | Acceptable | |
| Hydrocarbons - Aliphatic | Acceptable | Acceptable | |
| Hydrocarbons - Aromatic | Acceptable | Acceptable | |
| Inorganic Salt Solutions | Acceptable | Acceptable | |
| Ketones, Esters | Acceptable | Acceptable |
| Descriptive Properties | Value | Comments |
|---|---|---|
| Color | Natural | |
| Machinability | 3 | 1-10, 1=Easier to Machine |