Material Notes:
Type GA-50 combines high strength, toughness, wear resistance and damping capacity with excellent machinability. Responds well to heat treatment, local and surface hardening.General Meehanite information - Meehanite metal is first melted to a definite degree of undercooling or constitution which is related to the section of the casting to be poured and the range of physical properties such as tensile strength and hardness required. Nucleation with patented mixtures of graphitizing agents results in the removal of undercooling, in the controlled precipitation of graphite and in a fine grained eutectic cell structure which determines the density and physical integrity of the casting. Ordinary cast irons made to chemical specifications which do not include the benefit of controlled undercooling are influenced by mass effect to a maximum degree and for this and other reasons cannot be considered an equivalent to Meehanite metal.Information provided by Meehanite Marketing Association.
Physical Properties Metric English Comments
Specific Gravity 7.31 g/cc
7.31 g/cc
Mechanical Properties Metric English Comments
Hardness, Brinell 220
220
Nominal
Tensile Strength, Ultimate 345 MPa
50000 psi
Tensile Strength, Yield 152 MPa
22000 psi
.01% permanent set
Modulus of Elasticity 138 GPa
20000 ksi
Modulus of Rupture 0.621 GPa
90.0 ksi
Compressive Strength 1240 MPa
180000 psi
Poissons Ratio 0.32
0.32
Fatigue Strength 152 MPa
22000 psi
Machinability 48 %
48 %
Dalcher
Shear Modulus 60.3 GPa
8750 ksi
Shear Strength 345 MPa
50000 psi
Izod Impact Unnotched 33.9 - 47.5 J

@Diameter 20.3 mm
25.0 - 35.0 ft-lb

@Diameter 0.798 in
Thermal Properties Metric English Comments
CTE, linear 11.2 µm/m-°C

@Temperature 37.8 - 538 °C
6.20 µin/in-°F

@Temperature 100 - 1000 °F
Thermal Conductivity 50.4 W/m-K

@Temperature 10.0 - 232 °C
350 BTU-in/hr-ft²-°F

@Temperature 50.0 - 450 °F
Shrinkage 1.3 - 1.5 %
1.3 - 1.5 %
Patternmaker Shrinkage