Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

PolyOne Edgetek® NJ-30GF/000 natural Polyamide 12 (Nylon 12)

Category Polymer , Thermoplastic , Nylon , Nylon 12
Manufacturer PolyOne Corporation
Trade Name Edgetek®
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF PolyOne Edgetek® NJ-30GF/000 natural Polyamide 12 (Nylon 12).pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
The Edgetek® Engineering Thermoplastic Compounds portfolio covers a broad range of standard and custom-formulated high performance materials. This portfolio includes high-temperature materials for elevated service temperature environments, high-modulus / structural materials for load-bearing and high-strength applications and flame-retardant products. These compounds are based on selected engineering thermoplastic resins that are compounded with reinforcing additives such as carbon fiber, glass fiber and glass beads.Information provided by PolyOne
Physical Properties Metric English Comments
Linear Mold Shrinkage 0.0023 cm/cm
0.0023 in/in
ISO 294-4
Ash 30 %
30 %
Mechanical Properties Metric English Comments
Tensile Strength, Yield 106 MPa
15400 psi
ISO 527-2
Elongation at Break 2.5 %
2.5 %
ISO 527-2
Tensile Modulus 6.68 GPa
969 ksi
ISO 527-2
Charpy Impact Unnotched 5.00 J/cm²

@Temperature 23.0 °C
23.8 ft-lb/in²

@Temperature 73.4 °F
ISO 179
Charpy Impact, Notched 0.840 J/cm²

@Temperature 23.0 °C
4.00 ft-lb/in²

@Temperature 73.4 °F
ISO 179
Descriptive Properties Value Comments
Features General Purpose
Filler / Reinforcement Glass Fiber Reinforcement, 30% Filler by Weight
Forms Pellets
Generic Material Nylon 12
Generic Name Polyamide 12 (Nylon 12)
Regional Availability North America
Users viewing this material also viewed the following: