Material Notes:
Availability: North AmericaForms: PelletsAdditive: Heat Stabilizer and Impact ModifierFeatures: Heat Stabilized and Impact ModifiedProcessing Method: Injection MoldingInformation provided by TP Composites, Inc.
Physical Properties Metric English Comments
Density 1.03 g/cc
0.0372 lb/in³
ASTM D792
Melt Flow 1.5 g/10 min

@Load 3.80 kg,
Temperature 230 °C
1.5 g/10 min

@Load 8.38 lb,
Temperature 446 °F
ASTM D1238
4.0 g/10 min

@Load 10.0 kg,
Temperature 220 °C
4.0 g/10 min

@Load 22.0 lb,
Temperature 428 °F
ASTM D1238
Mechanical Properties Metric English Comments
Hardness, Rockwell R 95
95
ASTM D785
Tensile Strength 33.8 MPa
4900 psi
ASTM D638
Elongation at Yield 3.4 %
3.4 %
ASTM D638
Flexural Yield Strength 57.2 MPa
8300 psi
ASTM D790
Flexural Modulus 2.00 GPa
290 ksi
ASTM D790
Izod Impact, Notched 1.23 J/cm

@Thickness 3.17 mm,
Temperature -40.0 °C
2.30 ft-lb/in

@Thickness 0.125 in,
Temperature -40.0 °F
ASTM D256
2.40 J/cm

@Thickness 3.17 mm,
Temperature 0.000 °C
4.50 ft-lb/in

@Thickness 0.125 in,
Temperature 32.0 °F
ASTM D256
3.74 J/cm

@Thickness 3.17 mm,
Temperature 22.8 °C
7.00 ft-lb/in

@Thickness 0.125 in,
Temperature 73.0 °F
ASTM D256
Thermal Properties Metric English Comments
Deflection Temperature at 0.46 MPa (66 psi) 95.0 °C
203 °F
Unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 79.4 °C
175 °F
Unannealed; ASTM D648