Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Abatron AboCast/AboCure 8109-2

Category Polymer , Adhesive , Thermoset , Epoxy
Manufacturer Abatron
Trade Name AboCast/AboCure
Port Ningbo port,China
Trade Terms EXW, FOB, CFR, CIF
Payment Terms L/C, T/T, PayPal
Download PDF Abatron AboCast/AboCure 8109-2.pdf
Price EMAIL US    sales@lookpolymers.com
Material Notes:
High melting point. Filled version.Processing: 100/10 pbw; 90 minute potlife; mix at 130-140°C (270 °F); cures in 16 h/120°C (250°F), 10 h/140°C (285°F), 8 h/160°C (320°F), 2 h/ 200°C (390°F).Applications: Heavy duty casting and potting.
Physical Properties Metric English Comments
Density 1.75 g/cc
0.0632 lb/in³
Water Absorption 0.25 - 0.30 %
0.25 - 0.30 %
(60x10X4 mm bar) after 10 days at 20°C (77°F)
0.30 - 0.35 %
0.30 - 0.35 %
(60x10X4 mm bar) after 1 hour at 100°C (212°F)
Viscosity 5000 - 50000 cP
<br>@Temperature 120 °C
5000 - 50000 cP
<br>@Temperature 248 °F
Vapor Pressure <= 0.0000133 bar
<br>@Temperature 20.0 °C
<= 0.0100 torr
<br>@Temperature 68.0 °F
AboCure
<= 0.00133 bar
<br>@Temperature 180 °C
<= 1.00 torr
<br>@Temperature 356 °F
AboCast
0.00133 bar
<br>@Temperature 100 °C
1.00 torr
<br>@Temperature 212 °F
AboCure
0.00373 bar
<br>@Temperature 120 °C
2.80 torr
<br>@Temperature 248 °F
AboCure
0.0133 bar
<br>@Temperature 135 °C
10.0 torr
<br>@Temperature 275 °F
AboCure
Mechanical Properties Metric English Comments
Tensile Strength, Ultimate 62.05 MPa
9000 psi
Flexural Yield Strength 131 MPa
19000 psi
Compressive Yield Strength 193.1 MPa
28010 psi
Thermal Properties Metric English Comments
CTE, linear 30.0 - 35.0 µm/m-°C
<br>@Temperature 20.0 °C
16.7 - 19.4 µin/in-°F
<br>@Temperature 68.0 °F
Thermal Conductivity 0.590 - 0.670 W/m-K
4.09 - 4.65 BTU-in/hr-ft²-°F
Maximum Service Temperature, Air 115 °C
239 °F
Deflection temperature; load unknown
Electrical Properties Metric English Comments
Electrical Resistivity >= 1.50e+16 ohm-cm
>= 1.50e+16 ohm-cm
Dielectric Constant 3.7 - 4.0
<br>@Frequency 50 Hz
3.7 - 4.0
<br>@Frequency 50 Hz
3.9 - 4.2
<br>@Frequency 1000 Hz
3.9 - 4.2
<br>@Frequency 1000 Hz
4.0 - 4.2
<br>@Frequency 1e+6 Hz
4.0 - 4.2
<br>@Frequency 1e+6 Hz
Dielectric Strength 17.72 - 20.67 kV/mm
<br>@Thickness 3.17 mm
450.1 - 525.0 kV/in
<br>@Thickness 0.125 in
Short time value
Dissipation Factor 0.0090 - 0.014
<br>@Frequency 50 Hz
0.0090 - 0.014
<br>@Frequency 50 Hz
0.0090 - 0.015
<br>@Frequency 1000 Hz
0.0090 - 0.015
<br>@Frequency 1000 Hz
0.015 - 0.025
<br>@Frequency 1e+6 Hz
0.015 - 0.025
<br>@Frequency 1e+6 Hz
Processing Properties Metric English Comments
Processing Temperature 130 - 140 °C
266 - 284 °F
Pot Life 90.0 min
<br>@Temperature 120 °C
90.0 min
<br>@Temperature 248 °F
Copyright © lookpolymers.com All Rights Reserved