| Category | Polymer , Thermoplastic , Fluoropolymer , FEP , Fluorinated Ethylene Propylene (FEP), Molded/Extruded , PFA |
| Manufacturer | Daikin Industries |
| Trade Name | NEOFLON |
| Port | Shanghai port,China |
| Trade Terms | EXW, FOB, CFR, CIF |
| Payment Terms | L/C, T/T, PayPal |
| Download PDF | Daikin NEOFLON NP-101 FEP Pellets.pdf |
| Price | EMAIL US sales@lookpolymers.com |
| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Specific Gravity | 2.12 - 2.17 g/cc | 2.12 - 2.17 g/cc | ASTM D792 |
| Bulk Density | 1.20 g/cc | 0.0434 lb/in³ | |
| Water Absorption | <= 0.010 % @Thickness 8.50 mm, Time 86400 sec |
<= 0.010 % @Thickness 0.335 in, Time 24.0 hour |
ASTM D570 |
| Oxygen Transmission | 320 cc-mm/m²-24hr-atm | 812 cc-mil/100 in²-24hr-atm | at 25°C |
| Nitrogen Transmission | 104 cc-mm/m²-24hr-atm | 263 cc-mil/100 in²-24hr-atm | at 25°C |
| Viscosity | 4.00e+6 - 4.00e+7 cP @Temperature 380 °C |
4.00e+6 - 4.00e+7 cP @Temperature 716 °F |
Melt viscosity |
| Linear Mold Shrinkage | 0.030 - 0.060 cm/cm | 0.030 - 0.060 in/in | |
| Melt Flow | 21 - 27 g/10 min @Load 5.00 kg, Temperature 372 °C |
21 - 27 g/10 min @Load 11.0 lb, Temperature 702 °F |
|
| Deformation | 3.0 % | 3.0 % | 13.7 MPa load, at 25°C, 24 hrs; ASTM D621 |
| 5.0 % | 5.0 % | 6.7 MPa load, at 100°C, 24 hrs; ASTM D621 |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Hardness, Shore D | 55 | 55 | |
| Tensile Strength at Break | 19.0 - 22.0 MPa | 2760 - 3190 psi | ASTM D638 |
| Elongation at Break | 250 - 330 % | 250 - 330 % | ASTM D638 |
| Tensile Modulus | 0.343 GPa | 49.7 ksi | ASTM D638 |
| Flexural Modulus | 0.539 - 0.637 GPa | 78.2 - 92.4 ksi | ASTM D790 |
| Compressive Strength | 5.00 - 6.00 MPa @Temperature 25.0 °C |
725 - 870 psi @Temperature 77.0 °F |
1% deformation; ASTM D695 |
| Izod Impact, Unnotched | NB | NB | ASTM D256 |
| Coefficient of Friction | 0.040 - 0.060 | 0.040 - 0.060 | |
| Coefficient of Friction, Static | 0.050 | 0.050 | Coated-steel surface |
| Taber Abrasion, mg/1000 Cycles | <= 24 | <= 24 | Calculated using estimated density, 9.8 N load, cs-10 wheel |
| Thermal Properties | Metric | English | Comments |
|---|---|---|---|
| CTE, linear | 83.0 - 105 µm/m-°C @Temperature 23.0 - 60.0 °C |
46.1 - 58.3 µin/in-°F @Temperature 73.4 - 140 °F |
ASTM D696 |
| Thermal Conductivity | 0.250 W/m-K | 1.74 BTU-in/hr-ft²-°F | ASTM C177 |
| Melting Point | 250 - 260 °C | 482 - 500 °F | |
| Maximum Service Temperature, Air | 200 °C | 392 °F | Continuous use |
| Flammability, UL94 | V-0 | V-0 | |
| Oxygen Index | >= 95 % | >= 95 % | ASTM D2863 |
| Electrical Properties | Metric | English | Comments |
|---|---|---|---|
| Volume Resistivity | <= 1.00e+18 ohm-cm | <= 1.00e+18 ohm-cm | ASTM D257 |
| Dielectric Constant | 2.1 @Frequency 1000 Hz |
2.1 @Frequency 1000 Hz |
ASTM D150 |
| 2.1 @Frequency 1e+6 Hz |
2.1 @Frequency 1e+6 Hz |
ASTM D150 | |
| Dielectric Strength | 20.0 - 24.0 kV/mm @Thickness 3.20 mm |
508 - 610 kV/in @Thickness 0.126 in |
Short time; ASTM D149 |
| Dissipation Factor | 0.000060 @Frequency 1000 Hz |
0.000060 @Frequency 1000 Hz |
ASTM D150 |
| 0.00050 @Frequency 1e+6 Hz |
0.00050 @Frequency 1e+6 Hz |
ASTM D150 |
| Descriptive Properties | Value | Comments |
|---|---|---|
| Chemical Resistance | Excellent | |
| Contact Angle | 114 | Angle to level |
| Weatherability | Excellent |