Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

ExxonMobil AP3N Polypropylene Impact Copolymer

Category Polymer , Thermoplastic , Polypropylene (PP) , Polypropylene, Impact Modified; Molded/Extruded
Manufacturer Exxon Chemical
Trade Name
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF ExxonMobil AP3N Polypropylene Impact Copolymer.pdf
Price EMAIL US    sales@lookpolymers.com
Material Notes:
Product Description: A medium impact copolymer resin designed for appliance applications requiring good stiffness and fast cycle time.Availability: Asia Pacific Features:Fast Molding CycleHigh GlossHigh Stiffness Medium FlowMedium Impact ResistanceNucleated Uses: Appliance ComponentsAppliancesConsumer Applications Processing Method: Injection MoldingInformation provided by ExxonMobil
Physical Properties Metric English Comments
Density 0.900 g/cc
0.0325 lb/in³
ExxonMobil Method
Melt Flow 10 g/10 min

@Load 2.16 kg,
Temperature 230 °C
10 g/10 min

@Load 4.76 lb,
Temperature 446 °F
ASTM D1238
Mechanical Properties Metric English Comments
Tensile Strength, Yield 28.2 MPa
4090 psi
ISO 527-2/50
28.8 MPa
4180 psi
2.0 in/min; ASTM D638
Elongation at Yield 5.0 %
5.0 %
2.0 in/min; ASTM D638
5.0 %
5.0 %
ISO 527-2/50
Tensile Modulus 1.69 GPa
245 ksi
ISO527-2/1
Flexural Modulus 1.51 GPa
219 ksi
0.079 in/min; ISO 178
Flexural Modulus, 1% Secant 1480 MPa
215000 psi
0.05 in/min; ASTM D790A
1710 MPa
248000 psi
0.5 in/min; ASTM D790B
Izod Impact, Notched 0.961 J/cm

@Temperature 22.8 °C
1.80 ft-lb/in

@Temperature 73.0 °F
ASTM D256A
Izod Impact, Notched (ISO) 3.78 kJ/m²

@Temperature -40.0 °C
1.80 ft-lb/in²

@Temperature -40.0 °F
ISO 180/1A
4.62 kJ/m²

@Temperature -17.8 °C
2.20 ft-lb/in²

@Temperature 0.000 °F
ISO 180/1A
8.19 kJ/m²

@Temperature 22.8 °C
3.90 ft-lb/in²

@Temperature 73.0 °F
ISO 180/1A
Charpy Impact, Notched 0.357 J/cm²

@Temperature -30.0 °C
1.70 ft-lb/in²

@Temperature -22.0 °F
ISO 179/1eA
0.399 J/cm²

@Temperature -20.0 °C
1.90 ft-lb/in²

@Temperature -4.00 °F
ISO 179/1eA
0.462 J/cm²

@Temperature 0.000 °C
2.20 ft-lb/in²

@Temperature 32.0 °F
ISO 179/1eA
0.861 J/cm²

@Temperature 22.8 °C
4.10 ft-lb/in²

@Temperature 73.0 °F
ISO 179/1eA
Gardner Impact 18.0 J

@Thickness 3.17 mm,
Temperature -28.9 °C
13.2 ft-lb

@Thickness 0.125 in,
Temperature -20.0 °F
Geometry GC; ASTM D5420
Thermal Properties Metric English Comments
Deflection Temperature at 0.46 MPa (66 psi) 100 °C
212 °F
ISO 75-2/Bf
114 °C
237 °F
Unannealed; ASTM D648
123 °C
253 °F
Annealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 53.9 °C
129 °F
ISO 75-2/A