| Category | Polymer , Thermoplastic , Vinyl (PVC) , PVC, Rigid Grade |
| Manufacturer | PolyOne Corporation |
| Trade Name | Geon™ |
| Port | Shanghai port,China |
| Trade Terms | EXW, FOB, CFR, CIF |
| Payment Terms | L/C, T/T, PayPal |
| Download PDF | PolyOne Geon™ Vinyl Dry Blend E1354 Polyvinyl Chloride, Rigid (PVC, Rigid).pdf |
| Price | EMAIL US sales@lookpolymers.com |
| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Specific Gravity | 1.40 g/cc | 1.40 g/cc | ASTM D792 |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Tensile Strength, Yield | 48.6 MPa | 7050 psi | Type I, 5.1 mm/min; ASTM D638 |
| Tensile Modulus | 2.82 GPa | 409 ksi | Type I, 5.1 mm/min; ASTM D638 |
| Flexural Strength | 95.1 MPa | 13800 psi | ASTM D790 |
| Flexural Modulus | 3.23 GPa | 468 ksi | ASTM D790 |
| Izod Impact, Notched | 0.370 J/cm @Thickness 3.18 mm, Temperature 23.0 °C |
0.693 ft-lb/in @Thickness 0.125 in, Temperature 73.4 °F |
Compression Molded; ASTM D256A |
| Dart Drop Total Energy | 53.4 J/cm @Temperature 23.0 °C |
0.100 ft-lb/mil @Temperature 73.4 °F |
Procedure A, C.125; ASTM D4226 |
| 169 J/cm @Temperature 23.0 °C |
0.317 ft-lb/mil @Temperature 73.4 °F |
Procedure B, C.125; ASTM D4226 |
| Thermal Properties | Metric | English | Comments |
|---|---|---|---|
| CTE, linear, Parallel to Flow | 58.0 µm/m-°C | 32.2 µin/in-°F | ASTM D696 |
| Deflection Temperature at 1.8 MPa (264 psi) | 75.0 °C @Thickness 3.18 mm |
167 °F @Thickness 0.125 in |
Unannealed; ASTM D648 |
| Descriptive Properties | Value | Comments |
|---|---|---|
| Agency Ratings | CSA Unspecified Rating | |
| NSF 14 | ||
| NSF 61 | ||
| NSF Type I | ||
| Forms | Powder | |
| Generic Material | PVC, Rigid | |
| Generic Name | Polyvinyl Chloride, Rigid (PVC, Rigid) | |
| Processing Method | Extrusion | |
| PVC Cell Classification | 12454 | ASTM D1784 |
| Regional Availability | Africa & Middle East | |
| Asia Pacific | ||
| Europe | ||
| North America | ||
| South America | ||
| Uses | Piping |