| Category | Polymer , Thermoplastic , Polyester, TP , Polyethylene Terephthalate (PET) , PET-P Polyester, Extruded |
| Manufacturer | Quadrant Engineering Plastics Products |
| Trade Name | Ertalyte® |
| Port | Shanghai port,China |
| Trade Terms | EXW, FOB, CFR, CIF |
| Payment Terms | L/C, T/T, PayPal |
| Download PDF | Quadrant EPP Ertalyte® PET-P, Polyester-semi-crystalline thermoplastic, extruded (ASTM Product Data Sheet).pdf |
| Price | EMAIL US sales@lookpolymers.com |
| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Specific Gravity | 1.41 g/cc | 1.41 g/cc | ASTM D792 |
| Water Absorption | 0.070 % | 0.070 % | Immersion, 24hr; ASTM D570(2) |
| Water Absorption at Saturation | 0.90 % | 0.90 % | Immersion; ASTM D570(2) |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Hardness, Rockwell M | 93 | 93 | ASTM D785 |
| Hardness, Rockwell R | 125 | 125 | ASTM D785 |
| Hardness, Shore D | 87 | 87 | ASTM D2240 |
| Tensile Strength | 85.5 MPa | 12400 psi | ASTM D638 |
| Elongation at Break | 20 % | 20 % | ASTM D638 |
| Tensile Modulus | 3.17 GPa | 460 ksi | ASTM D638 |
| Flexural Strength | 124 MPa | 18000 psi | ASTM D790 |
| Flexural Modulus | 3.38 GPa | 490 ksi | ASTM D790 |
| Compressive Strength | 103 MPa | 15000 psi | 10% Def.; ASTM D695 |
| Compressive Modulus | 2.90 GPa | 420 ksi | ASTM D695 |
| Shear Strength | 55.2 MPa | 8000 psi | ASTM D732 |
| Izod Impact, Notched | 0.267 J/cm | 0.500 ft-lb/in | ASTM D256 Type A |
| Coefficient of Friction, Dynamic | 0.20 | 0.20 | Dry vs. Steel; QTM55007 |
| K (wear) Factor | 121 x 10<sup>-8</sup> mm³/N-M | 60.0 x 10<sup>-10</sup> in³-min/ft-lb-hr | QTM 55010 |
| Limiting Pressure Velocity | 0.0981 MPa-m/sec | 2800 psi-ft/min | 4:1 safety factor; QTM 55007 |
| Thermal Properties | Metric | English | Comments |
|---|---|---|---|
| CTE, linear | 59.4 µm/m-°C @Temperature -40.0 - 149 °C |
33.0 µin/in-°F @Temperature -40.0 - 300 °F |
ASTM E831 |
| Thermal Conductivity | 0.288 W/m-K | 2.00 BTU-in/hr-ft²-°F | ASTM F433 |
| Melting Point | 255 °C | 491 °F | Crystalline, Peak; ASTM D3418 |
| Maximum Service Temperature, Air | 98.9 °C | 210 °F | Long Term |
| Deflection Temperature at 1.8 MPa (264 psi) | 116 °C | 240 °F | ASTM D648 |
| Flammability, UL94 | HB | HB | 1/8 inch (Estimated Rating) |
| Electrical Properties | Metric | English | Comments |
|---|---|---|---|
| Surface Resistivity per Square | >= 1.00e+13 ohm | >= 1.00e+13 ohm | EOS/ESD S11.11 |
| Dielectric Constant | 3.4 @Frequency 1e+6 Hz |
3.4 @Frequency 1e+6 Hz |
ASTM D150 |
| Dielectric Strength | 15.2 kV/mm | 385 kV/in | Short Term; ASTM D149 |
| Dissipation Factor | 0.020 @Frequency 1e+6 Hz |
0.020 @Frequency 1e+6 Hz |
ASTM D150 |
| Compliance Properties | Metric | English | Comments |
|---|---|---|---|
| 3A-Dairy | Yes | Yes | Natural Only |
| Canada AG | Yes | Yes | Natural Only |
| FDA | Yes | Yes | |
| NSF | No | No | |
| USDA | Yes | Yes | |
| USP Class VI | No | No |
| Chemical Resistance Properties | Metric | English | Comments |
|---|---|---|---|
| Acids, Strong (pH 1-3) | Limited | Limited | |
| Acids, Weak | Acceptable | Acceptable | |
| Alcohols | Acceptable | Acceptable | |
| Alkalies, Strong (pH 11-14) | Unacceptable | Unacceptable | |
| Alkalies, Weak | Acceptable | Acceptable | |
| Chlorinated Solvents | Unacceptable | Unacceptable | |
| Conductive / Static Dissipative | No | No | |
| Continuous Sunlight | Limited | Limited | |
| Hot Water / Steam | Limited | Limited | |
| Hydrocarbons - Aliphatic | Acceptable | Acceptable | |
| Hydrocarbons - Aromatic | Acceptable | Acceptable | |
| Inorganic Salt Solutions | Acceptable | Acceptable | |
| Ketones, Esters | Acceptable | Acceptable |
| Descriptive Properties | Value | Comments |
|---|---|---|
| Color | Natural and black | |
| Machinability | 2 | 1-10, 1=Easier to Machine |