| Category | Polymer , Thermoplastic , Polyketone , Polyetheretherketone (PEEK) , Polyetheretherketone, PEEK, Glass Fiber Filled |
| Manufacturer | Quadrant Engineering Plastics Products |
| Trade Name | Ketron® |
| Port | Ningbo port,China |
| Trade Terms | EXW, FOB, CFR, CIF |
| Payment Terms | L/C, T/T, PayPal |
| Download PDF | Quadrant EPP Ketron® GF30 LSG PEEK, Extruded 30% Glass-Reinforced Polyetherether Ketone (ASTM Product Data Sheet).pdf |
| Price | EMAIL US sales@lookpolymers.com |
| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Specific Gravity | 1.51 g/cc | 1.51 g/cc | ASTM D792 |
| Water Absorption | 0.10 % | 0.10 % | Immersion, 24hr; ASTM D570 |
| Water Absorption at Saturation | 0.30 % | 0.30 % | ASTM D570 |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Hardness, Rockwell M | 103 | 103 | ASTM D785 |
| Hardness, Rockwell R | 126 | 126 | ASTM D785 |
| Hardness, Shore D | 89 | 89 | ASTM D2240 |
| Ball Indentation Hardness | 215 MPa | 31200 psi | ISO 2039-1 |
| Tensile Strength | 96.5 MPa | 14000 psi | ASTM D638 |
| Elongation at Break | 2.0 % | 2.0 % | ASTM D638 |
| Tensile Modulus | 6.89 GPa | 1000 ksi | ASTM D638 |
| Flexural Strength | 159 MPa | 23000 psi | ASTM D790 |
| Flexural Modulus | 6.89 GPa | 1000 ksi | ASTM D790 |
| Compressive Strength | 152 MPa | 22000 psi | 10% Def.; ASTM D695 |
| Compressive Modulus | 3.79 GPa | 550 ksi | ASTM D695 |
| Shear Strength | 96.5 MPa | 14000 psi | |
| Izod Impact, Notched | 0.427 J/cm | 0.800 ft-lb/in |
| Thermal Properties | Metric | English | Comments |
|---|---|---|---|
| CTE, linear | 21.6 µm/m-°C @Temperature -40.0 - 149 °C |
12.0 µin/in-°F @Temperature -40.0 - 300 °F |
ASTM E831 |
| Thermal Conductivity | 0.429 W/m-K | 2.98 BTU-in/hr-ft²-°F | |
| Melting Point | 340 °C | 644 °F | ASTM D3418 |
| Maximum Service Temperature, Air | 249 °C | 480 °F | |
| Deflection Temperature at 1.8 MPa (264 psi) | 232 °C | 450 °F | ASTM D648 |
| Flammability, UL94 | V-0 @Thickness 3.00 mm |
V-0 @Thickness 0.118 in |
| Electrical Properties | Metric | English | Comments |
|---|---|---|---|
| Surface Resistivity per Square | >= 1.00e+13 ohm | >= 1.00e+13 ohm | IEC 60093 |
| Dielectric Strength | 19.7 kV/mm | 500 kV/in |
| Compliance Properties | Metric | English | Comments |
|---|---|---|---|
| 3A-Dairy | No | No | |
| Canada AG | No | No | |
| FDA | No | No | |
| NSF | No | No | |
| USDA | No | No | |
| USP Class VI | Yes | Yes |
| Chemical Resistance Properties | Metric | English | Comments |
|---|---|---|---|
| Acids, Strong (pH 1-3) | Limited | Limited | |
| Acids, Weak | Acceptable | Acceptable | |
| Alcohols | Acceptable | Acceptable | |
| Alkalies, Strong (pH 11-14) | Acceptable | Acceptable | |
| Alkalies, Weak | Acceptable | Acceptable | |
| Chlorinated Solvents | Acceptable | Acceptable | |
| Conductive / Static Dissipative | No | No | |
| Continuous Sunlight | Limited | Limited | |
| Hot Water / Steam | Acceptable | Acceptable | |
| Hydrocarbons - Aliphatic | Acceptable | Acceptable | |
| Hydrocarbons - Aromatic | Acceptable | Acceptable | |
| Inorganic Salt Solutions | Acceptable | Acceptable | |
| Ketones, Esters | Acceptable | Acceptable |
| Descriptive Properties | Value | Comments |
|---|---|---|
| Color | Natural |