Thermal Properties | Metric | English | Comments |
---|---|---|---|
Thermal Conductivity | 21.5 W/m-K @Temperature 500 °C |
149 BTU-in/hr-ft²-°F @Temperature 932 °F |
|
Haynes Ultimet® alloy, aged 1000 hours at 649°C (1200°F) Co content as balance, excellent corrosion resistance, outstanding wear resistance, high tensile strength combined with excellent impact toughness and ductility. Ideal welding material with exceptio.. |
|||
Thermal Conductivity | 21.5 W/m-K @Temperature 500 °C |
149 BTU-in/hr-ft²-°F @Temperature 932 °F |
|
Haynes Ultimet® alloy, aged 1000 hours at 871°C (1600°F) Co content as balance, excellent corrosion resistance, outstanding wear resistance, high tensile strength combined with excellent impact toughness and ductility. Ideal welding material with exceptio.. |
|||
Thermal Conductivity | 21.5 W/m-K @Temperature 500 °C |
149 BTU-in/hr-ft²-°F @Temperature 932 °F |
|
Haynes Ultimet® alloy, all-weld metal, GMAW weld (short) Co content as balance, excellent corrosion resistance, outstanding wear resistance, high tensile strength combined with excellent impact toughness and ductility. Ideal welding material with exceptio.. |
|||
Thermal Conductivity | 21.5 W/m-K @Temperature 500 °C |
149 BTU-in/hr-ft²-°F @Temperature 932 °F |
|
Haynes Ultimet® alloy, all-weld metal, GTAW weld Co content as balance, excellent corrosion resistance, outstanding wear resistance, high tensile strength combined with excellent impact toughness and ductility. Ideal welding material with exceptio.. |
|||
Thermal Conductivity | 21.5 W/m-K @Temperature 500 °C |
149 BTU-in/hr-ft²-°F @Temperature 932 °F |
|
Haynes Ultimet® alloy, mill annealed Co content as balance, excellent corrosion resistance, outstanding wear resistance, high tensile strength combined with excellent impact toughness and ductility. Ideal welding material with exceptio.. |
|||
Thermal Conductivity | 21.5 W/m-K @Temperature 500 °C |
149 BTU-in/hr-ft²-°F @Temperature 932 °F |
|
Haynes Ultimet® alloy, plate, GMAW weld (short) Co content as balance, excellent corrosion resistance, outstanding wear resistance, high tensile strength combined with excellent impact toughness and ductility. Ideal welding material with exceptio.. |
|||
Thermal Conductivity | 21.5 W/m-K @Temperature 500 °C |
149 BTU-in/hr-ft²-°F @Temperature 932 °F |
|
Haynes Ultimet® alloy, plate, GMAW weld (spray) Co content as balance, excellent corrosion resistance, outstanding wear resistance, high tensile strength combined with excellent impact toughness and ductility. Ideal welding material with exceptio.. |
|||
Thermal Conductivity | 21.5 W/m-K @Temperature 800 °C |
149 BTU-in/hr-ft²-°F @Temperature 1470 °F |
|
Haynes 625SQ® Nickel Alloy Sheet Haynes 625SQ alloy is a solid-solution strengthened superalloy. It is a modification of Haynes 625 alloy designed to enhance resistance to fatigue at temperatures up to approximately 1200°F (649Â.. |
|||
Thermal Conductivity | 21.4 W/m-K @Temperature 600 °C |
149 BTU-in/hr-ft²-°F @Temperature 1110 °F |
|
Haynes Hastelloy® G-30® alloy, 12.7 mm (1/2 in.) thick plate, GMAW spray weld 1.1 mm diameter filler wire HASTELLOY® G-30® alloy is a high chromium nickel-base alloy which shows superior corrosion resistance in commercial phosphoric acids as well as many complex environments containing highly oxid.. |
|||
Thermal Conductivity | 21.4 W/m-K @Temperature 600 °C |
149 BTU-in/hr-ft²-°F @Temperature 1110 °F |
|
Haynes Hastelloy® G-30® alloy, 3.2 mm thick sheet, GTAW weld HASTELLOY® G-30® alloy is a high chromium nickel-base alloy which shows superior corrosion resistance in commercial phosphoric acids as well as many complex environments containing highly oxid.. |
|||
Thermal Conductivity | 21.4 W/m-K @Temperature 600 °C |
149 BTU-in/hr-ft²-°F @Temperature 1110 °F |
|
Haynes Hastelloy® G-30® alloy, 30% cold rolled HASTELLOY® G-30® alloy is a high chromium nickel-base alloy which shows superior corrosion resistance in commercial phosphoric acids as well as many complex environments containing highly oxid.. |
|||
Thermal Conductivity | 21.4 W/m-K @Temperature 600 °C |
149 BTU-in/hr-ft²-°F @Temperature 1110 °F |
|
Haynes Hastelloy® G-30® alloy, 50% cold rolled and 1 hour at 500°C, air cooled HASTELLOY® G-30® alloy is a high chromium nickel-base alloy which shows superior corrosion resistance in commercial phosphoric acids as well as many complex environments containing highly oxid.. |
|||
Thermal Conductivity | 21.4 W/m-K @Temperature 600 °C |
149 BTU-in/hr-ft²-°F @Temperature 1110 °F |
|
Haynes Hastelloy® G-30® alloy, 50% cold rolled and 5000 hours at 500°C, air cooled HASTELLOY® G-30® alloy is a high chromium nickel-base alloy which shows superior corrosion resistance in commercial phosphoric acids as well as many complex environments containing highly oxid.. |
|||
Thermal Conductivity | 21.4 W/m-K @Temperature 600 °C |
149 BTU-in/hr-ft²-°F @Temperature 1110 °F |
|
Haynes Hastelloy® G-30® alloy, 6.4 mm thick plate HASTELLOY® G-30® alloy is a high chromium nickel-base alloy which shows superior corrosion resistance in commercial phosphoric acids as well as many complex environments containing highly oxid.. |
|||
Thermal Conductivity | 21.4 W/m-K @Temperature 600 °C |
149 BTU-in/hr-ft²-°F @Temperature 1110 °F |
|
Haynes Hastelloy® G-30® alloy, plate and bar HASTELLOY® G-30® alloy is a high chromium nickel-base alloy which shows superior corrosion resistance in commercial phosphoric acids as well as many complex environments containing highly oxid.. |
|||
Thermal Conductivity | 21.4 W/m-K @Temperature 500 °C |
149 BTU-in/hr-ft²-°F @Temperature 932 °F |
|
AK Steel 201LN Austenitic Stainless steel AK Steel 210 was developed originally to conserve nickel. It provides properties similar to Type 301 and can be used in most applications for Type 301. This alloy is non-magnetic in the annealed c.. |
|||
Thermal Conductivity | 21.4 W/m-K @Temperature 500 °C |
149 BTU-in/hr-ft²-°F @Temperature 932 °F |
|
AK Steel 304L Austenitic Stainless steel AK Steel 304L is an extra low-carbon variation of Type 304, that eliminates carbide precipitation due to welding. AK Steel 304L can be used in the "as-welded" condition, even in severe corrosive co.. |
|||
Thermal Conductivity | 21.5 W/m-K @Temperature 200 °C |
149 BTU-in/hr-ft²-°F @Temperature 392 °F |
|
Assab Steels ASSAB XW-5 Cold Work Steel ASSAB XW-5 is a high-carbon, high chromium tool steel alloyed with tungsten, characterized by:High wear resistanceHigh compressive strengthHigh surface hardness after hardeningGood through-hardening.. |
|||
Thermal Conductivity | 21.4 W/m-K @Temperature 500 °C |
149 BTU-in/hr-ft²-°F @Temperature 932 °F |
|
ATI Allegheny Ludlum Stainless Steel Chromium-Nickel Type 304, 10% Cold Rolled (UNS S30400) This alloy is one of the most familiar and most frequently used alloy in the stainless steel family. It may be best used in applications where the following properties are important: resistance to .. |
|||
Thermal Conductivity | 21.4 W/m-K @Temperature 500 °C |
149 BTU-in/hr-ft²-°F @Temperature 932 °F |
|
ATI Allegheny Ludlum Stainless Steel Chromium-Nickel Type 304, 50% Cold Rolled (UNS S30400) This alloy is one of the most familiar and most frequently used alloy in the stainless steel family. It may be best used in applications where the following properties are important: resistance to .. |
|||
Thermal Conductivity | 21.4 W/m-K @Temperature 500 °C |
149 BTU-in/hr-ft²-°F @Temperature 932 °F |
|
ATI Allegheny Ludlum Stainless Steel Chromium-Nickel Type 304L, 50% Cold Rolled (UNS S30403) This alloy is one of the most familiar and most frequently used alloy in the stainless steel family. It may be best used in applications where the following properties are important: resistance to .. |
|||
Thermal Conductivity | 21.4 W/m-K @Temperature 500 °C |
149 BTU-in/hr-ft²-°F @Temperature 932 °F |
|
ATI Allegheny Ludlum Stainless Steel Chromium-Nickel Type 304L, 60% Cold Rolled (UNS S30403) This alloy is one of the most familiar and most frequently used alloy in the stainless steel family. It may be best used in applications where the following properties are important: resistance to .. |
|||
Thermal Conductivity | 21.4 W/m-K @Temperature 500 °C |
149 BTU-in/hr-ft²-°F @Temperature 932 °F |
|
ATI Allegheny Ludlum Stainless Steel Chromium-Nickel Type 304L, Annealed (UNS S30403) This alloy is one of the most familiar and most frequently used alloy in the stainless steel family. It may be best used in applications where the following properties are important: resistance to .. |
|||
Thermal Conductivity | 21.4 W/m-K @Temperature 500 °C |
149 BTU-in/hr-ft²-°F @Temperature 932 °F |
|
ATI Allegheny Ludlum Stainless Steel Chromium-Nickel Type 302, 10% Cold Rolled (UNS S30200) This alloy is one of the most familiar and most frequently used alloy in the stainless steel family. It may be best used in applications where the following properties are important: resistance to .. |
|||
Thermal Conductivity | 21.4 W/m-K @Temperature 500 °C |
149 BTU-in/hr-ft²-°F @Temperature 932 °F |
|
ATI Allegheny Ludlum Stainless Steel Chromium-Nickel Type 304, 30% Cold Rolled (UNS S30400) This alloy is one of the most familiar and most frequently used alloy in the stainless steel family. It may be best used in applications where the following properties are important: resistance to .. |
|||
Thermal Conductivity | 21.4 W/m-K @Temperature 500 °C |
149 BTU-in/hr-ft²-°F @Temperature 932 °F |
|
ATI Allegheny Ludlum Stainless Steel Chromium-Nickel Type 304, Annealed (UNS S30400) This alloy is one of the most familiar and most frequently used alloy in the stainless steel family. It may be best used in applications where the following properties are important: resistance to .. |
|||
Thermal Conductivity | 21.4 W/m-K @Temperature 500 °C |
149 BTU-in/hr-ft²-°F @Temperature 932 °F |
|
ATI Allegheny Ludlum Stainless Steel Chromium-Nickel Type 305, 0% Cold Rolled (UNS S30500) This alloy is one of the most familiar and most frequently used alloy in the stainless steel family. It may be best used in applications where the following properties are important: resistance to .. |
|||
Thermal Conductivity | 21.4 W/m-K @Temperature 500 °C |
149 BTU-in/hr-ft²-°F @Temperature 932 °F |
|
ATI Allegheny Ludlum Stainless Steel Chromium-Nickel Type 305, 20% Cold Rolled (UNS S30500) This alloy is one of the most familiar and most frequently used alloy in the stainless steel family. It may be best used in applications where the following properties are important: resistance to .. |
|||
Thermal Conductivity | 21.4 W/m-K @Temperature 600 °C |
149 BTU-in/hr-ft²-°F @Temperature 1110 °F |
|
Haynes Hastelloy® G-30® alloy, 10% cold rolled HASTELLOY® G-30® alloy is a high chromium nickel-base alloy which shows superior corrosion resistance in commercial phosphoric acids as well as many complex environments containing highly oxidizin.. |
|||
Thermal Conductivity | 21.4 W/m-K @Temperature 600 °C |
149 BTU-in/hr-ft²-°F @Temperature 1110 °F |
|
Haynes Hastelloy® G-30® alloy, 12.7 mm (1/2 in.) thick plate HASTELLOY® G-30® alloy is a high chromium nickel-base alloy which shows superior corrosion resistance in commercial phosphoric acids as well as many complex environments containing highly oxidizin.. |