CoorsTek AD-996 99.6% Alumina

Category Ceramic , Oxide , Aluminum Oxide
Manufacturer CoorsTek
Trade Name
Port Shanghai port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF CoorsTek AD-996 99.6% Alumina.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
Physical Properties Metric English Comments
Density 3.90 g/cc
0.141 lb/in³
ASTM-C 20
Particle Size 6.0 µm
6.0 µm
Average Crystal Size; THIN-SECTION
Mechanical Properties Metric English Comments
Hardness, Rockwell 45 N 83
83
Modulus of Elasticity 370 GPa
53700 ksi
ASTM-C848
Flexural Strength 379 MPa
55000 psi
MOR; ASTM-F417
Compressive Strength 2600 MPa
377000 psi
ASTM-C773
Poissons Ratio 0.22
0.22
ASTM-C848
Fracture Toughness 4.00 - 5.00 MPa-m½
3.64 - 4.55 ksi-in½
Klc; Notched Beam
Shear Modulus 152 GPa
22000 ksi
Calculated
Thermal Properties Metric English Comments
CTE, linear 8.20 µm/m-°C

@Temperature 25.0 - 1000 °C
4.56 µin/in-°F

@Temperature 77.0 - 1830 °F
ASTM-C372
Thermal Conductivity 30.0 W/m-K
208 BTU-in/hr-ft²-°F
ASTM-C408
Maximum Service Temperature, Air 1750 °C
3180 °F
NO-LOAD COND.
Component Elements Properties Metric English Comments
Al2O3 99.6 %
99.6 %
Nominal
Electrical Properties Metric English Comments
Volume Resistivity 2.00e+6 ohm-cm

@Temperature 1000 °C
2.00e+6 ohm-cm

@Temperature 1830 °F
ASTM-D1829
2.00e+10 ohm-cm

@Temperature 500 °C
2.00e+10 ohm-cm

@Temperature 932 °F
ASTM-D1829
>= 1.00e+14 ohm-cm

@Temperature 25.0 °C
>= 1.00e+14 ohm-cm

@Temperature 77.0 °F
ASTM-D1829
Descriptive Properties Value Comments
Color Ivory
Thermal Shock Resistance (°C) 200
ΔTc