Eastman Tritan EX401 Copolyester

Category Polymer , Thermoplastic , Polyester, TP
Manufacturer Eastman Chemical
Trade Name Tritan
Port Ningbo port,China
Trade Terms FOB, CFR, CIF
Payment Terms L/C, T/T, Western Union
Download PDF Eastman Tritan EX401 Copolyester.pdf
Price EMAIL US    sales@lookpolymers.com
  Online Service   lookpolymers   27660005
Material Notes:
Eastman Tritan EX401 is an amorphous copolyester with excellent appearance and clarity. Tritan EX401 contains a mold release derived from vegetable based sources. Its most outstanding features are excellent toughness, hydrolytic stability, and heat and chemical resistance. Tritan EX401 was specifically developed for the infant care market using Eastman's knowledge of copolyester chemistry. Tritan EX401 can be converted into parts using injection molding and extrusion blow molding techniques.Application/UsesInfant CareKey AttributesEase of ProcessingExcellent clarityExcellent hydrolytic stabilityGood chemical resistanceGood heat resistanceOutstanding impact resistanceInformation was provided by Eastman.
Physical Properties Metric English Comments
Specific Gravity 1.17 g/cc
1.17 g/cc
ASTM D792
Linear Mold Shrinkage 0.0050 - 0.0070 cm/cm
0.0050 - 0.0070 in/in
ASTM D955
Mechanical Properties Metric English Comments
Hardness, Rockwell R 115
115
ASTM D785
Tensile Strength at Break 53.0 MPa
7690 psi
ASTM D638
Tensile Strength, Yield 44.0 MPa
6380 psi
ASTM D638
Elongation at Break 140 %
140 %
ASTM D638
Elongation at Yield 7.0 %
7.0 %
ASTM D638
Flexural Yield Strength 66.0 MPa
9570 psi
ASTM D790
Flexural Modulus 1.585 GPa
229.9 ksi
ASTM D790
Izod Impact, Notched 1.26 J/cm

@Temperature -40.0 °C
2.36 ft-lb/in

@Temperature -40.0 °F
ASTM D256
6.50 J/cm

@Temperature 23.0 °C
12.2 ft-lb/in

@Temperature 73.4 °F
ASTM D256
Izod Impact, Unnotched NB

@Temperature 23.0 °C
NB

@Temperature 73.4 °F
ASTM D4812
NB

@Temperature -40.0 °C
NB

@Temperature -40.0 °F
ASTM D4812
Puncture Energy 59.0 J

@Temperature 23.0 °C
43.5 ft-lb

@Temperature 73.4 °F
Energy @ Max. Load; ASTM D3763
63.0 J

@Temperature -40.0 °C
46.5 ft-lb

@Temperature -40.0 °F
Energy @ Max. Load; ASTM D3763
Thermal Properties Metric English Comments
Deflection Temperature at 0.46 MPa (66 psi) 109 °C
228 °F
ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 92.0 °C
198 °F
ASTM D648
Optical Properties Metric English Comments
Haze <= 1.0 %
<= 1.0 %
ASTM D1003
Transmission, Visible 92 %
92 %
ASTM D1003
Compliance Properties Metric English Comments
FDA Yes
Yes
Repeated use food contact articles
Processing Properties Metric English Comments
Processing Temperature 260 - 282 °C
500 - 540 °F
Mold Temperature 38.0 - 66.0 °C
100 - 151 °F
Drying Temperature 88.0 °C
190 °F
Dry Time 4 - 6 hour
4 - 6 hour