Material Notes:
A clay with excellent kaolin content and virtually no carbon content. It is highly plastic with excellent fired brightness and is an excellent clay for a variety of ceramic glaze and porcelain compositions.Information provided by Old Hickory Clay Company
Physical Properties Metric English Comments
Particle Size 0.46 µm
0.46 µm
Median particle diameter
0.50 µm
0.50 µm
56% of particles less than
1.0 µm
1.0 µm
68% of particles less than
<= 5.0 µm
<= 5.0 µm
89% of particles less than
pH 5.8
5.8
Soluble Sulfates 150 ppm
150 ppm
Specific Surface Area 21.4 m²/g
21.4 m²/g
Mechanical Properties Metric English Comments
Modulus of Rupture 0.00345 GPa
0.500 ksi
Dry Modulus of Rupture, 50% clay/50% flint, cast bars
Thermal Properties Metric English Comments
Shrinkage 6.58 %
6.58 %
Linear Drying Shrinkage
Component Elements Properties Metric English Comments
Al2O3 29.47 %
29.47 %
CaO 0.10 %
0.10 %
Fe2O3 1.11 %
1.11 %
K2O 0.51 %
0.51 %
Loss on Ignition(%) 9.86 %
9.86 %
MgO 0.35 %
0.35 %
Na2O 0.080 %
0.080 %
SiO2 56.47 %
56.47 %
TiO2 2.08 %
2.08 %
Descriptive Properties Value Comments
CEC/MBI (meg/100 ml) 7.4
Crude Color Light Grey
Filtration (ml) 25
Water of Plasticity (%) 35.5
Wet Sieve Residue (%) 0.29
Wet Sieve Residue, +200 mesh