Material Notes:
ALC is the same material as ZAL-15 - but brings exceptional uniformity in an insulation material in cylindrical form.Information provided by Zircar Ceramics.
Physical Properties Metric English Comments
Density 0.240 g/cc
0.00867 lb/in³
Open Porosity 93 %
93 %
Mechanical Properties Metric English Comments
Flexural Strength 0.689 MPa

@Strain 60.0 %
100 psi

@Strain 60.0 %
Load applied normal to fiber plane, strain = load deformation in mils; Three Point Bending, sample 0.5"*0.5"*4"
0.689 MPa

@Strain 40.0 %
100 psi

@Strain 40.0 %
Load applied parallel to fiber plane, strain = load deformation in mils; Three Point Bending, sample 0.5"*0.5"*4"
Compressive Yield Strength 0.0689 MPa

@Strain 8.00 %
10.0 psi

@Strain 8.00 %
Load applied normal to fiber plane
0.0827 MPa

@Strain 4.00 %
12.0 psi

@Strain 4.00 %
Load applied normal to fiber plane
0.207 MPa

@Strain 4.00 %
30.0 psi

@Strain 4.00 %
Load applied parallel to fiber plane
0.345 MPa

@Strain 8.00 %
50.0 psi

@Strain 8.00 %
Load applied parallel to fiber plane
Thermal Properties Metric English Comments
CTE, linear 5.00 µm/m-°C

@Temperature 20.0 - 1000 °C
2.78 µin/in-°F

@Temperature 68.0 - 1830 °F
Specific Heat Capacity 1.05 J/g-°C
0.250 BTU/lb-°F
Thermal Conductivity 0.0700 W/m-K

@Temperature 400 °C
0.486 BTU-in/hr-ft²-°F

@Temperature 752 °F
parallel to thickness; ASTM C177-76
0.130 W/m-K

@Temperature 800 °C
0.902 BTU-in/hr-ft²-°F

@Temperature 1470 °F
Parallel to Thickness; ASTM C177-76
0.190 W/m-K

@Temperature 1100 °C
1.32 BTU-in/hr-ft²-°F

@Temperature 2010 °F
Parallel to Thickness; ASTM C177-76
0.260 W/m-K

@Temperature 1400 °C
1.80 BTU-in/hr-ft²-°F

@Temperature 2550 °F
Parallel to Thickness; ASTM C177-76
0.280 W/m-K

@Temperature 1650 °C
1.94 BTU-in/hr-ft²-°F

@Temperature 3000 °F
Parallel to Thickness; ASTM C177-76
Melting Point 1870 °C
3400 °F
Maximum Service Temperature, Air 1550 °C
2820 °F
Continuous
1650 °C
3000 °F
Intermittent
Shrinkage 1.00 %

@Temperature 1550 °C,
Time 3600 sec
1.00 %

@Temperature 2820 °F,
Time 1.00 hour
Perpendicular to Thickness
3.00 %

@Temperature 1650 °C,
Time 3600 sec
3.00 %

@Temperature 3000 °F,
Time 1.00 hour
Perpendicular to Thickness
Component Elements Properties Metric English Comments
Al2O3 85 %
85 %
SiO2 15 %
15 %
Descriptive Properties Value Comments
Bond Silica
Color White