Songhan Plastic Technology Co.,Ltd.
 POLYMER SEARCH

Polymer Property : Maximum Service Temperature, Air = 190 °C Product List

Thermal Properties

Tips: 30 items are displayed at most.
Thermal Properties Metric English Comments
Maximum Service Temperature, Air 190 °C
374 °F
Intermittent
Nylacast Nylube GF Cast Nylon 6, Lubricated (Blended Solid and Liquid Lubricant), Glass Filled
For applications requiring higher compressive strength the NYLUBE GF masterbatch incorporates hollow glass ovule, designed to float and evenly distribute through the polymerising polymer. The glass ..
Maximum Service Temperature, Air 190 °C
374 °F
Short Time; IEC 60216
PolyOne Bergamid™ B650 G/Mi20 UF Polyamide 6 (Nylon 6)
Information provided by PolyOne
Maximum Service Temperature, Air 190 °C
374 °F
Short Time; IEC 60216
PolyOne Bergamid™ B700 G20 H UF Polyamide 6 (Nylon 6)
Information provided by PolyOne
Maximum Service Temperature, Air 190 - 232 °C
374 - 450 °F
Average value: 208 °C Grade Count:24
Overview of materials for Phenolic, Novolac, Mineral Filled
This property data is a summary of similar materials in the MatWeb database for the category "Phenolic, Novolac, Mineral Filled". Each property range of values reported is minimum and maximum values..
Maximum Service Temperature, Air 190 °C
374 °F
Menzolit Menzolit® BMC 1500 Unsaturated Polyester UP
BMC 1500 is a special BMC for the use at elevated temperature. The glass content is set to a level that combines good flowability with good strength and stiffness properties. Even without a specific..
Maximum Service Temperature, Air 190 °C
374 °F
Menzolit Menzolit® SMC 1500 Unsaturated Polyester UP
SMC 1500 is a special SMC for applications calling for high continuous service temperature. The glass level has been selected to combine good mouldability with good strength and stiffness properties..
Maximum Service Temperature, Air 190 °C
<br>@Time >=1800 sec
374 °F
<br>@Time >=0.500 hour
Congo Red; BS 2782
Teknor Apex Sinvicomp SFW 8000 Polyvinyl Chloride, Flexible
Availability: Asia Pacific Uses: Footwear; General Purpose Forms: Pellets Processing Method: Injection MoldingInformation Provided by Teknor Apex
Maximum Service Temperature, Air 190 °C
<br>@Time Error in fixSigDigits: @digits must be between 1 a sec
374 °F
<br>@Time Error in fixSigDigits: @digits must be between 1 a hour
Congo Red; BS 2782
Teknor Apex Sinvicomp SGH 5500G Polyvinyl Chloride, Flexible
Availability: Asia Pacific Uses: Garden Hose Forms: Pellets Processing Method: ExtrusionInformation Provided by Teknor Apex
Maximum Service Temperature, Air 190 °C
<br>@Time >=1800 sec
374 °F
<br>@Time >=0.500 hour
Congo Red; BS 2782
Teknor Apex Sinvicomp SGH 7000 Polyvinyl Chloride, Flexible
Availability: Asia Pacific Uses: Garden Hose Forms: Pellets Processing Method: ExtrusionInformation Provided by Teknor Apex
Maximum Service Temperature, Air 190 °C
<br>@Time >=1800 sec
374 °F
<br>@Time >=0.500 hour
ASTM D2115-92
Teknor Apex Sinvicomp SHE 4000 Polyvinyl Chloride, Flexible
Availability: Asia Pacific Features: Ethylene Oxide Sterilizable Uses: Medical/Healthcare Applications Forms: Pellets Processing Method: ExtrusionInformation Provided by Teknor Apex
Maximum Service Temperature, Air 190 °C
<br>@Time >=1800 sec
374 °F
<br>@Time >=0.500 hour
Congo Red; ASTM D2115-92
Teknor Apex Sinvicomp SHM 4200 Polyvinyl Chloride, Flexible
Availability: Asia Pacific Features: Ethylene Oxide Sterilizable Uses: Medical/Healthcare Applications Forms: Pellets Processing Method: Injection MoldingInformation Provided by Teknor Apex
Maximum Service Temperature, Air 190 °C
<br>@Time >=1800 sec
374 °F
<br>@Time >=0.500 hour
Congo Red; BS 2782
Teknor Apex Sinvicomp SFE 5500 Polyvinyl Chloride, Flexible
Availability: Asia Pacific Features: Food Contact Acceptable; Non-Toxic Uses: Hose; Tubing Forms: Pellets Processing Method: ExtrusionInformation Provided by Teknor Apex
Maximum Service Temperature, Air 190 °C
<br>@Time >=Error in fixSigDigits: @digits must be between 1 a sec
374 °F
<br>@Time >=Error in fixSigDigits: @digits must be between 1 a hour
Congo Red; BS 2782
Teknor Apex Sinvicomp SFE 6000 Polyvinyl Chloride, Flexible
Availability: Asia Pacific Features: Food Contact Acceptable; Non-Toxic Uses: Hose; Tubing Forms: Pellets Processing Method: ExtrusionInformation Provided by Teknor Apex
Maximum Service Temperature, Air 190 °C
<br>@Time >=3600 sec
374 °F
<br>@Time >=1.00 hour
Congo Red; BS 2782
Teknor Apex Sinvicomp SFW 5000 Polyvinyl Chloride, Flexible
Availability: Asia Pacific Uses: Footwear; General Purpose Forms: Pellets Processing Method: Injection MoldingInformation Provided by Teknor Apex
Maximum Service Temperature, Air 190 °C
<br>@Time >=Error in fixSigDigits: @digits must be between 1 a sec
374 °F
<br>@Time >=Error in fixSigDigits: @digits must be between 1 a hour
Congo Red; BS 2782
Teknor Apex Sinvicomp SFW 6000 Polyvinyl Chloride, Flexible
Availability: Asia Pacific Uses: Footwear; General Purpose Forms: Pellets Processing Method: Injection MoldingInformation Provided by Teknor Apex
Maximum Service Temperature, Air 190 °C
<br>@Time >=1800 sec
374 °F
<br>@Time >=0.500 hour
ASTMD 2115-92
Teknor Apex Sinvicomp SMG 6500 Polyvinyl Chloride, Flexible
Availability: Asia Pacific Features: Food Contact Acceptable; Non-Toxic Uses: Toys Forms: Pellets Processing Method: Injection MoldingInformation Provided by Teknor Apex
Maximum Service Temperature, Air 190 °C
<br>@Time >=Error in fixSigDigits: @digits must be between 1 a sec
374 °F
<br>@Time >=Error in fixSigDigits: @digits must be between 1 a hour
Congo Red; BS 2782
Teknor Apex Sinvicomp SPF 8020 Polyvinyl Chloride, Flexible
Availability: Asia Pacific Features: Good Stiffness Uses: Gaskets; Profiles; Seals Forms: Pellets Processing Method: ExtrusionInformation Provided by Teknor Apex
Maximum Service Temperature, Air 190 °C
<br>@Time >=7200 sec
374 °F
<br>@Time >=2.00 hour
Congo Red; BS 2782
Teknor Apex Sinvicomp SRF 2703 Polyvinyl Chloride, Rigid
Availability: Asia Pacific Features: Good Weather Resistance; Good Impact Resistance Uses: Fittings Forms: Pellets Processing Method: Injection MoldingInformation Provided by Teknor Apex
Maximum Service Temperature, Air 190 °C
<br>@Time >=1800 sec
374 °F
<br>@Time >=0.500 hour
Congo Red; BS 2782
Teknor Apex Sinvicomp SRF 3704 Polyvinyl Chloride, Rigid
Availability: Asia Pacific Features: High Impact Resistance Uses: Fittings Forms: Pellets Processing Method: Injection MoldingInformation Provided by Teknor Apex
Maximum Service Temperature, Air 190 °C
<br>@Time 1800 sec
374 °F
<br>@Time 0.500 hour
Congo Red; BS 2782
Teknor Apex Sinvicomp SRF 9702/C Polyvinyl Chloride, Rigid
Availability: Asia Pacific Features: Medium Impact Resistance Uses: Electrical/Electronic Applications Forms: Pellets Processing Method: Injection MoldingInformation Provided by Teknor Apex
Maximum Service Temperature, Air 190 °C
<br>@Time >=1800 sec
374 °F
<br>@Time >=0.500 hour
Congo Red; BS 2782
Teknor Apex Sinvicomp SRP 5906 Polyvinyl Chloride, Rigid
Availability: Asia Pacific Features: Medium Impact Resistance Uses: Conduit; Piping; Profiles Forms: Pellets Processing Method: ExtrusionInformation Provided by Teknor Apex
Maximum Service Temperature, Air 190 °C
<br>@Time >=3600 sec
374 °F
<br>@Time >=1.00 hour
Congo Red; BS 2782
Teknor Apex Sinvicomp SSG 6006 Polyvinyl Chloride, Flexible
Availability: Asia Pacific Features: Good Flexibility Uses: Cable Jacketing; Wire and Cable Applications Wire Types: ST4; ST5; Type 6; YM1; YM2 Agency Ratings: BS 6746; IEC 60227; VDE 0207 Forms: P..
Maximum Service Temperature, Air 190 °C
<br>@Time >=7200 sec
374 °F
<br>@Time >=2.00 hour
Congo Red; BS 2782
Teknor Apex Sinvicomp SSH 5509 Polyvinyl Chloride, Flexible
Availability: Asia Pacific Features: Good Flexibility Uses: Cable Jacketing; Wire and Cable Applications Wire Types: ST1; ST2; Type 9; Class 1/3 Agency Ratings: BS 6746; IEC 60502; JIS 6723 Forms: ..
Maximum Service Temperature, Air 190 °C
374 °F
Continuous
Wolf Kunststoff ZEDEX® ZX-410V7T A4T Polymer Alloy, Fiber Reinforced, Friction Modified
Main Characteristics: Fiber-reinforced; Friction-modified; Very high stiffness (higher than that of fiber-reinforced PEEK); Very low thermal expansion coefficient; Low friction; High wear resistance..
Maximum Service Temperature, Air 190 °C
374 °F
Tra-Con Tra-Bond 2248 High Temperature Epoxy Staking Adhesive
TRA-BOND 2248 is a thixotropic, high temperature cure, 100% solids epoxy resin system that provides strong, tough bonds between a wide range of materials (includes metals, glass, ceramics, and many ..
Maximum Service Temperature, Air 190 °C
374 °F
Tra-Con Tra-Duct 2924 Conductive Silver Epoxy Adhesive
TRA-DUCT 2924 is a two part electrically conductive composition developed for low shrinkage, low resistivity bonding applications where good electrical and physical properties over a wide temperatur..
Maximum Service Temperature, Air 190 °C
374 °F
Dow Corning MOLYKOTE® PG-21 PLASTISLIP GREASE
Silicone grease especially for plastic/plastic and plastic/metal combinations like control cables and circuit lever systemInformation provided by Dow Corning
Maximum Service Temperature, Air 190 °C
374 °F
ChevronTexaco Delo® Synthetic Grease SF
FeaturesChevron Delo Synthetic Grease SF is a high performance grease specifically engineered for trailer wheel-ends operating in all conditions, even under the most extreme high and low temperature..
Maximum Service Temperature, Air 190 °C
374 °F
Two Hour Heat Resistance per ASTM D648
Chang Chun Plastic Longlite PM T310 Impact Phenolic Molding Compound
ASTM Grade per ASTM D700 is 13.Information provided by Dowell Trading Company Ltd.
Maximum Service Temperature, Air 190 °C
374 °F
Heat Resistance; ASTM D570D
Plenco 7591 Phenolic, Pellet, Transfer Molded
PLENCO 07591 is a mineral and flock cotton filled novolac phenolic molding compound. UL recognized under component file E40654.Information supplied by Plenco.
Copyright © lookpolymers.com All Rights Reserved