| Category | Polymer , Thermoplastic , Nylon , Nylon 6 , Nylon 6, 50% Glass Fiber Filled |
| Manufacturer | A. Schulman, Inc. |
| Trade Name | SCHULAMID® |
| Port | Shanghai port,China |
| Trade Terms | EXW, FOB, CFR, CIF |
| Payment Terms | L/C, T/T, PayPal |
| Download PDF | A. Schulman SCHULAMID® 6 GF50H 50% Glass Fiber Reinforced Nylon 6.pdf |
| Price | EMAIL US sales@lookpolymers.com |
| Physical Properties | Metric | English | Comments |
|---|---|---|---|
| Specific Gravity | 1.55 g/cc | 1.55 g/cc | ISO 1183/1 |
| Linear Mold Shrinkage | 0.0010 cm/cm @Thickness 3.175 mm |
0.0010 in/in @Thickness 0.1250 in |
ASTM D955 |
| Mechanical Properties | Metric | English | Comments |
|---|---|---|---|
| Tensile Strength at Break | 210 MPa | 30400 psi | ISO 527 |
| Tensile Modulus | 16.0 GPa | 2320 ksi | ISO 527 |
| Izod Impact, Notched | 1.44 J/cm | 2.70 ft-lb/in | ASTM D256 |
| Thermal Properties | Metric | English | Comments |
|---|---|---|---|
| Deflection Temperature at 0.46 MPa (66 psi) | 215 °C | 419 °F | ISO 75 |
| Deflection Temperature at 1.8 MPa (264 psi) | 210 °C | 410 °F | ASTM D648 |
| Processing Properties | Metric | English | Comments |
|---|---|---|---|
| Melt Temperature | 270 - 295 °C | 518 - 563 °F | |
| Mold Temperature | 65.6 - 93.3 °C | 150 - 200 °F | |
| Drying Temperature | 79.4 °C | 175 °F | |
| Dry Time | 2 - 4 hour | 2 - 4 hour | Predrying |
| Moisture Content | 0.080 - 0.12 % | 0.080 - 0.12 % |